Table 4. Salt Spray Resistance of Cured IBImIL/ImILA Epoxy Systems and their Adhesion Strengths at 40–50 °C in Seawater Fog Humidity >99%.
| disbonded
area |
adhesion
strengths (MPa) |
|||||
|---|---|---|---|---|---|---|
| sample no. | exposure time (h) | cm2 | % | ASTM D1654-92 rating | before salt spray | after salt spray exposure time |
| IBImIL/ImILA | 0 | 0 | 0 | 10 | 14.5 ± 0.01 | 14.5 ± 0.02 |
| 1000 | 0.4 ± 0.003 | 1 ± 0.002 | 10 | 14.5 ± 0.03 | 13.8 ± 0.04 | |
| 1200 | 1.2 ± 0.001 | 1 ± 0.001 | 9 | 14.5 ± 0.02 | 13.0 ± 0.06 | |
| 1500 | 2.1 ± 0.002 | 3 ± 0.003 | 8 | 14.5 ± 0.04 | 10.8 ± 0.02 | |
| 2000 | 13 ± 0.01 | 11 ± 0.01 | 6 | 14.5 ± 0.01 | 6.8 ± 0.02 | |