Skip to main content
. 2023 Apr 26;10(5):522. doi: 10.3390/bioengineering10050522

Table 1.

High-resolution XPS scan data for the different surface treatments, (i) untreated, (ii) air-plasma-treated, (iii) acrylic-acid-plasma-coated, (iv) fibronectin-coated, (v) air-plasma-treated and fibronectin-coated, and (vi) acrylic-acid-plasma-coated and fibronectin-coated.

C1s C-C/C-H at%
(285 eV)
C-O/C-N at%
(286.2 eV)
(C,N)-C=O at%
(288.2 eV)
HO-C=O at%
(288.9 eV)
Untreated 67.6 ± 0.1 19.1 ± 0.3 2.1 ± 0.2 11.3 ± 0.1
Air plasma 62.8 ± 3.0 22.4 ± 2.4 1.8 ± 0.4 13.1 ± 1.0
AAc plasma 56.3 ± 1.7 28.0 ±2.0 1.2 ± 0.1 14.6 ± 0.2
Untreated and fibronectin 61.4 ± 0.3 23.6 ± 0.3 4.1± 0.2 10.9 ± 0.9
Air plasma and fibronectin 52.7 ±2.6 29.3 ± 2.7 6.1 ± 0.1 11.8 ± 0.1
AAc plasma and fibronectin 55.6 ± 0.4 28.7 ± 0.3 6.2 ± 0.6 9.6 ± 0.5