Skip to main content
. 2023 Jun 24;9(7):e17627. doi: 10.1016/j.heliyon.2023.e17627

Table 4.

FSW parameters of the PLA Plus and HDPE for welded.

No Pin Profile Tool speed (rpm) Traverse speed (mm/min) Material UTS (MPa) Weld efficieny (%)
Base PLA Plus 30.72
Base HDPE 30.5
1 Triangle 1000 30 PLA Plus/PLA Plus 31.93 103.94
2 Triangle 1000 50 14.95 48.67
3 Triangle 1500 30 42.12 136.99
4 Triangle 1500 50 39.39 128.11
5 Square 1000 30 30.19 98.27
6 Square 1000 50 23.03 74.86
7 Square 1500 30 28.7 93.42
8 Square 1500 50 32.09 104.46
9 Triangle 1000 30 HDPE/HDPE 16.27 53.34
10 Triangle 1000 50 19.69 64.56
11 Triangle 1500 30 17.75 58.2
12 Triangle 1500 50 7.63 25.02
13 Square 1000 30 17.38 56.98
14 Square 1000 50 11.19 36.69
15 Square 1500 30 20.34 66,69
16 Square 1500 50 13.21 43.31
17 Triangle 1000 30 PLA Plus/HDPE
18 Triangle 1000 50
19 Triangle 1500 30
20 Triangle 1500 50
21 Square 1000 30
22 Square 1000 50
23 Square 1500 30
24 Square 1500 50

UTS: Ultimate Tensile Strength.