The composition of furan-based copolyesters was determined from 1H NMR and SECa.
| Copolymer | Composition | 1H NMRb | SECc | |||
|---|---|---|---|---|---|---|
| Theoretical wt% [mol%] | Calculatedb wt% [mol%] | M n [g mol−1] | M n [g mol−1] | M w [g mol−1] | Đ | |
| PHF-DLF | 70/30 [86.6/13.4] | 67.5/32.5 [85.2/14.8] | 17 600 | 5700 | 10 700 | 1.9 |
| POF-DLF | 70/30 [85.3/14.7] | 68.1/31.9 [84.2/15.8] | 19 500 | 13 700 | 40 500 | 3.0 |
| PDF-DLF | 70/30 [84.0/16.0] | 70.0/30.0 [84.0/16.0] | 23 900 | 19 000 | 42 600 | 2.2 |
| PDDF-DLF | 70/30 [82.8/17.2] | 70.7/29.3 [83.2/16.8] | 34 800 | 20 600 | 45 700 | 2.2 |
M n – number average molecular mass, Mw – weight average molecular mass, Đ – dispersity index.
Values calculated from 1H NMR.