Table 1.
Comparison of four months aged PSMPs with freshly prepared PSMPs, regarding particle size determined by DLS, zeta potential, emission spectra, and PLQY.
![]() Unstained PSMPs |
![]() QD-loaded, polymerization |
![]() QD-loaded, swelling |
|
|---|---|---|---|
| Particle size by DLS in µm | |||
| After synthesis | 2.00 ± 0.25 | 2.46 ± 0.40 | 2.69 ± 0.51 |
| After four months | 1.88 ± 0.15 | 1.78 ± 0.13 | 1.07 ± 0.17 |
| Zeta potential by DLS in mV | |||
| After synthesis | − 48 ± 2 | − 49 ± 1 | − 22 ± 2 |
| After four months | − 40 ± 4 | − 40 ± 1 | − 24 ± 3 |
| PLQY in % | |||
| After synthesis | / | 24% | 48% |
| After four months | / | 15% | 31% |
| Emission spectra | / | ![]() |
![]() |