Skip to main content
. 2023 Jul 20;9(8):e18524. doi: 10.1016/j.heliyon.2023.e18524

Table 4.

Functional groups and the corresponding wavenumber in the MA and VA monomers, PPMA, PPVA and PP(MA-VA) thin films.

Assignment MA Wavenumber (cm−1)
VA Band intensity
PP(MA-VA)
PPMA 3:1 1:1 1:3 PPVA
O H stretching 3438 3443 3442 3470 3443 3444 3443 Broad peak
C H3 stretching 2961 2980 Merged
C H2 stretching 2938 2926 2928 2928 2922 2918 2938 Sharp
C H stretching 2862 2860 2860 2860 2860 2860 2860 Merged
C = O stretching 1734 1709 1702 1700 1700 1705 1741 Broad peak
C Created by potrace 1.16, written by Peter Selinger 2001-2019 C stretching 1645 1636 1635 1634 1635 1633 1638 Very low
CH3 bending 1464 1448 1448 1445 1448 1445 1436 Merged
CH2 bending 1385 1380 1380 1380 1379 1379 1375 Low
C O 1282, 1243, Sharp peak
1128 1167 1122 1269 1156 1200 1125 Merged
C Created by potrace 1.16, written by Peter Selinger 2001-2019 C bending 1024 1024 1031 1030 1027 1023 1025 low merged
863 852 860 800 Low
C H out of plane bending 676 674 681 678 660 685 648 Low