Table 1.
Summary of the research on poly-based electromagnetic shielding composites with uniform structure.
| Materials * | Filler Loading | EMI SE (dB) | Thickness (mm) | Frequency | Ref. |
|---|---|---|---|---|---|
| PVA/GN/Fe3O4 | 0.1 wt% | 40.7 | 0.2 | 8–12 Ghz | [79] |
| EP/PES/MWCNT | 2.9 wt% | 23 | 2.2 | 8–12 Ghz | [80] |
| GN/CFN | 20 wt% | 73 | 2 | 8–12 Ghz | [72] |
| VGCNF/PVDF | 5 wt% | 16.4 | 0.82 | 30 Khz–1.5 Ghz | [81] |
| PEDOT/GNP | 15 wt% | 18 | - | 8–12 Ghz | [82] |
| RGO/PdNi/EVA | 1 wt% | 30 | - | 8–12 Ghz | [83] |
| POM/MWCNT | 40 wt% | 45.7 | 0.15 | 8–12 Ghz | [75] |
| PE/PVDF/Fe3O4/CNT | 10 wt% | 26 | 2.6 | 18–26 Ghz | [84] |
| PLLA/MWCNT | 10 vol% | 23 | 2.5 | 8–12 Ghz | [85] |
| PVDF/RGO | 21 wt% | 60 | 1.5 | 8–12 Ghz | [74] |
| PLA/PEO/GNP | 6 wt% | 10.5 | - | 8–12 Ghz | [86] |
| PMMA/GNP-MWCNT | 8 wt% | 36 | 2 | 8–12 Ghz | [87] |
| PDMS/GA | 12.5 wt% | 52 | 3 | 4–16 Ghz | [88] |
| PVDF/Ba4CO2Fe36O60 | 20 wt% | 83 | 0.12 | 8–18 Ghz | [89] |
| CF/PAA/Fe3O4 | 10 wt% | 40.6 | 3.5 | 2–18 Ghz | [90] |
| PVDF/PANI | 30 wt% | 65 | 1 | 8–12 Ghz | [73] |
| ABS/CB/CNT | 3 wt% | 29 | 2 | 8–12 Ghz | [91] |
| PP/MWCNT | 20 wt% | 47 | 2 | 8–12 Ghz | [92] |
| BF/PANI | 7 wt% | 35.73 | - | 8–12 Ghz | [93] |
| PS/PANI | 40 wt% | 45 | 0.25 | 8–12 Ghz | [71] |
| CB/EMA/TPO | 30 wt% | 29 | 1 | 14–20 Ghz | [94] |
| PLA/CNT | 5.6 wt% | 31.1 | - | 8–12 Ghz | [95] |
| SWCNT/PANI | 3 wt% | 32.8 | 0.5 | 8–12 Ghz | [96] |
| TPU/SiAPP/SCF/Ti3C2Tx MXene | 20 wt% | 50.5 | 1 | 8–12 Ghz | [97] |
* GN—graphene; PVA—polyvinyl alcohol; CFN—carbon fiber network; VGCNF—vapor-grown carbon nanofiber; PE—polyethylene; PLLA—poly (l-lactic acid); PLA—polylactic acid; PEO—poly(ethylene oxide); GA—graphene aerogel; CF—carbon fiber; PAA—polyacrylic acid; PP—polypropylene; BF—Bagasse Fiber.