Table 8. Measurement of Test Samples: Ultimate/Breaking Load, Lap Shear Strength, and Flexural Strength.
Sample No. | TRS, rpm | DT, Sec | PR,mm/min | Ultimate/Breaking Load, N | Lap Shear Strength, MPa | Flexural Strength, MPa |
---|---|---|---|---|---|---|
1 | 1500 | 8 | 4 | 2224 | 78.37 | 144.85 |
2 | 1500 | 8 | 8 | 2142 | 75.47 | 154.36 |
3 | 1500 | 8 | 12 | 2041 | 72.04 | 158.69 |
4 | 1500 | 16 | 4 | 2189 | 77.27 | 169.45 |
5 | 1500 | 16 | 8 | 2373 | 83.76 | 161.32 |
6 | 1500 | 16 | 12 | 2442 | 84.70 | 155.26 |
7 | 1500 | 24 | 4 | 2652 | 98.61 | 135.67 |
8 | 1500 | 24 | 8 | 1994 | 70.38 | 169.66 |
9 | 1500 | 24 | 12 | 2055 | 72.54 | 171.32 |
10 | 1900 | 8 | 4 | 2158 | 76.17 | 177.45 |
11 | 1900 | 8 | 8 | 2454 | 86.46 | 178.48 |
12 | 1900 | 8 | 12 | 2525 | 88.97 | 177.00 |
13 | 1900 | 16 | 4 | 2142 | 75.61 | 187.75 |
14 | 1900 | 16 | 8 | 3022 | 106.67 | 197.85 |
15 | 1900 | 16 | 12 | 3041 | 107.34 | 188.96 |
16 | 1900 | 24 | 4 | 2960 | 104.48 | 187.35 |
17 | 1900 | 24 | 8 | 2845 | 100.42 | 187.85 |
18 | 1900 | 24 | 12 | 2554 | 88.59 | 179.55 |
19 | 2300 | 8 | 4 | 2640 | 93.19 | 179.75 |
20 | 2300 | 8 | 8 | 2789 | 98.45 | 179.25 |
21 | 2300 | 8 | 12 | 2852 | 100.67 | 169.60 |
22 | 2300 | 16 | 4 | 2751 | 97.11 | 166.99 |
23 | 2300 | 16 | 8 | 1854 | 65.44 | 160.65 |
24 | 2300 | 16 | 12 | 1953 | 68.94 | 155.45 |
25 | 2300 | 24 | 4 | 2171 | 76.63 | 149.85 |
26 | 2300 | 24 | 8 | 2094 | 73.91 | 150.65 |
27 | 2300 | 24 | 12 | 2078 | 73.35 | 155.80 |