Table 1.
The lattice constant a (Å), crystallite size R (nm), strain, dislocation density (nm−2), x-ray density DXRD (g/cm3), measured density (g/cm3), porosity P and bond lengths (Å) between cations and anions in tetrahedral (A) and octahedral (B) sites of MgFe2O4.
| a (Å) | R (nm) | (nm-2) | DXRD (g/cm3) | (g/cm3) | |
|---|---|---|---|---|---|
|
8.3826 |
35.55 |
1.3 × 10−3 |
7.9 × 10−4 |
4.51 |
2.14 |
| P (%) | LA-A (Å) | LA-B (Å) | LB-B (Å) | LA-O (Å) | LB-O (Å) |
| 53 | 3.6298 | 3.4752 | 2.9637 | 1.6472 | 3.7975 |