Skip to main content
. 2023 Sep 19;6(19):17986–17995. doi: 10.1021/acsanm.3c03247

Table 1. Basic Characteristics of the SWCNT BP and Nonwoven SWCNT–TPU Composite Sheets.

    recovered SWCNT–TPU nanocomposite sheets
  volume fraction (vol %)
sample name SWCNT/TPU wt. ratio in solvent SWCNT/TPU (wt % ratio) thickness (μm) density (g cm–3) SWCNT TPU void
SWCNT BP 1:0 100:0 78 0.31 17 0 83
SWCNT-TPU-90 1:0.1 90:10 88 0.32 16 3 81
SWCNT-TPU-80 1:0.25 80:20 92 0.35 15 7 78
SWCNT-TPU-50 1:1.5 50:50 100 0.55 15 24 62
SWCNT-TPU-35 1:2.5 35:65 137 0.51 10 28 62
SWCNT-TPU-20 1:5 20:80 190 0.61 7 40 52
SWCNT-TPU-17 1:7 17:83 145 1.02 10 71 19
SWCNT-TPU-12 1:10 12:88 243 0.94 6 69 24
SWCNT-TPU-8 1:15 8:92 432 0.91 4 71 25
SWCNT-TPU-5 1:20 5:95 590 0.92 3 73 24