sample E (MPa) σfail (MPa) εfail (%) Gt (MJ/m3) Gε=40% (MJ/m3)
SWCNT BP 270 ± 30 3 ± 0.4 3.3 ± 0.7 0.09 ± 0.03  
SWCNT-TPU-90 576 ± 75 14 ± 1 11 ± 1 1.1 ± 0.1  
SWCNT-TPU-80 955 ± 81 22 ± 4 13 ± 2 2 ± 0.6  
SWCNT-TPU-50 1773 ± 91 80 ± 3 41 ± 1 23 ± 1 21 ± 0.9
SWCNT-TPU-35 1068 ± 57 61 ± 2 47 ± 14 19 ± 4 14 ± 2
SWCNT-TPU-20 839 ± 31 60 ± 3 57 ± 5 23 ± 3 13 ± 0.5
SWCNT-TPU-17 1517 ± 117 73 ± 5 62 ± 4 33 ± 5 17 ± 0.8
SWCNT-TPU-12 828 ± 72 50 ± 3 73 ± 17 27 ± 7 11 ± 0.3
SWCNT-TPU-8 469 ± 28 39 ± 1 106 ± 14 31 ± 5 7 ± 0.3
TPU 160 ± 14 18 ± 2 764 ± 126 94 ± 20 3 ± 0.1