DSC parameters and output for material characterization.

Fiber characterization (material code) Samples masses (mg) Heating rate (°C/min) Heating range (°C) Average Tg (°C) Average Tm (°C) Average Tc (°C)
Highly oriented PET (M1) 2.6, 2.47, 2.68 10 20 to 270 80.92 252.36
Polypropylene PP (M2) 2.85, 3.14 10 −50 to 200 −36.43 163.62
Pre-oriented PET (M3A) 3.93, 3.59, 4.18 10 20 to 280 69.86 243.14 110.7
Highly oriented PET (M3B) 3.06, 3.54, 3.95, 3.79 10 20 to 270 80.95 252.4