PV dehydration of ethanol through various polymeric membranes.

Polymer Feed
(wt.% Ethanol)
Temperature (°C) Separation Factor Flux
(g/m2h)
Ref.
Polyacrylonitrile-polyvinylpyrrolidone 96 20 3.2 2200 [58]
Poly(acrylic acid-co-acrylonitrile) 82 15 877 13 [59]
Poly(vinyl chloride) 96 40 63 3 [60]
Cellulose acetate 96 60 5.9 200 [61]
PVA/25% TEOS, annealed at 160 °C 85 40 329 5 [61]
PVA/25% TEOS, annealed at 130 °C 85 40 893 4 [61]
Chitosan 96 40 2208 4 [62]