Skip to main content
. 2023 Oct 31;15(21):4282. doi: 10.3390/polym15214282

Table 3.

Maximum temperature (Tm) and weight loss percentage (%) for PVA/Cs/ZnO nanocomposites.

Sample Stage I Stage II Stage III Stage IV Residual
Mass
Ti (°C)
Tm
°C
Weight
(%)
Tm
°C
Weight (%) Tm
°C
Weight (%) Tm
°C
Weight (%)
PVA/Cs 100.3 4.19 179.7 10.15 271.9 41.16 507.8 40.61 4.15 142
PVA/Cs/2 wt% ZnO 92.30 3.29 179.8 8.67 273.3 40.44 502.2 39.36 8.72 161
PVA/Cs/5 wt% ZnO 100.6 3.46 207.6 10.50 265.1 40.38 508.8 27.66 8.21 164
PVA/Cs/10 wt% ZnO 108.4 2.76 253.9 47.42 486.4 37.45 --- --- 12.37 178
PVA/Cs/15 wt% ZnO 108.3 1.68 250.5 42.22 478.1 34.80 --- --- 22.44 210