Skip to main content
. 2023 Dec 1;13:21230. doi: 10.1038/s41598-023-48191-5

Table 7.

Handsheet properties of BS soda pulp blended with TOCC.

Sample (BS: TOCC) CSF (mL) Tensile index (N m/g) Burst index (kPa m2/g) Ring crush index (kgf m2/g) Bulk (cm3/g)
BS TOCC
100 0 350 43.40 ± 1.52c 2.54 ± 0.06d 12.86 ± 0.51c 2.08 ± 0.03c
50 50 395 30.15 ± 0.95a 1.68 ± 0.05c 10.66 ± 0.44b 2.00 ± 0.03b
0 100 385 28.62 ± 1.70a 1.03 ± 0.05a 9.29 ± 0.04a 1.79 ± 0.06a
JOCC 405 32.85 ± 2.063b 1.37 ± 0.09b 10.24 ± 0.32 b 1.76 ± 0.03a
The quality requirement standard for corrugated board paper in CNS
Corrugating medium (CNS 1455 B-grade)  > 29.43  > 7
Liner board (CNS 2955 C-grade) 2.0  > 10

Comparison of the data for different groups was performed by using Turkey’s HSD test. The significant level is set at p ≤ 0.05; Group a < b < c < d.