Table 6.
Conversion of PP-ol to corresponding products using various catalysts.
| Catalyst | PP-ol | PP-one | Ph-CHO | Ph-OCHO | Ph-OH | Ph-COCH3 | Experimental conditions | References |
|---|---|---|---|---|---|---|---|---|
| TiO2 (homemade) |
12 | 1 | – | – | – | – | 10 mg of catalyst, 1 mL of CH3CN, 455 nm, 10 h | [43] |
| Pd/TiO2 |
19 | – | – | – | – | – | 0.1 mmol of PP-ol, 5 mg of catalyst, 1.0 mL of CH3CN, 455 nm, 42 °C, 4 h. The | [26] |
| VOSO4 | 44.6 | 44.6 | – | – | – | – | Substrate (0.5 mmol), catalyst (0.1 mmol, MeOH (2 mL), O2(0.4 MPa), 100 °C, 12 h | [44] |
| Zn4In2S7-GO | 38.5 | 34.3 | – | 2.3 | 1.85 | 0.1 mmol of PP-ol, 0.01 g of catalyst, O2, 5 mL of CH3CN, 300 W Xe-lamp, for 2 h. |
[45] |
|
| TiO2 P25 | 69 | 6.2 | 25 | 29 | 20 | – | 1 mM, 15 mL of PP-ol solution, 15 mg of catalyst, UV, 6 h, 30 °C | This study |
| TiO2 US22-B |
57 | 10.1 | 42 | 20 | 3 | – | 1 mM, 15 mL of PP-ol solution, 15 mg of catalyst, UV, 6 h, 30 °C | This study |