Size (diameter – D), absorption band and band gap of ZnO nanoparticles.

Sample FESEM UV-Vis XRD
D (nm) l max (nm) Band gap (eV) Scherrer method W–H method
D (nm) ε graphic file with name d3ra08928b-t3.jpg R 2 D (nm)
A1 60–90 381 2.15 34.0 0.0014 0.00414 0.9718 33.5
A2 60–120 383 2.0 28.6 0.0025 0.00473 0.9807 29.3
A3 30–120 376 1.8 32.6 0.0022 0.00459 0.9790 30.2
B1 30–90 375 2.65 33.9 0.0015 0.00444 0.9079 31.2
B2 30–90 378 2.2 26.3 0.0025 0.00425 0.9875 32.6
B3 40–60 384 2.3 28.7 0.0019 0.00490 0.9788 28.3
C1 20–60 380 2.35 30.5 0.0015 0.00446 0.9402 31.2
C2 20–40 376 2.15 24.0 0.0029 0.00531 0.9849 26.1
C3 30–50 375 2.1 22.9 0.0026 0.00592 0.9919 23.4