Skip to main content
. 2024 Aug 22;14:19509. doi: 10.1038/s41598-024-70189-w

Table 3.

Experimental parametric amalgamations produced through the RSM model, and their wear results.

L (N) V (m/s) D (m) SWR (mm3/Nm)
10 2.5 1250 0.0000855811 ± 2.57 × 10–6
16 3.4 1696 0.000119 ± 3.57 × 10–6
16 1.6 1696 0.000102746 ± 3.08 × 10–6
16 3.4 804 0.00012207 ± 3.6621 × 10–6
16 1.6 804 0.0000722456 ± 2.17 × 10–6
25 2.5 1250 0.000146653 ± 4.40 × 10–6
25 2.5 1250 0.000166836 ± 5.01 × 10–6
25 1 1250 0.000142238 ± 4.27 × 10–6
25 2.5 1250 0.000181015 ± 5.43 × 10–6
25 2.5 2000 0.000197691 ± 5.93 × 10–6
25 4 1250 0.000181775 ± 5.45 × 10–6
25 2.5 1250 0.000169735 ± 5.09 × 10–6
25 2.5 1250 0.000172497 ± 5.17 × 10–6
25 2.5 500 0.000155115 ± 4.65 × 10–6
25 2.5 1250 0.000168709 ± 5.06 × 10–6
34 1.6 1696 0.00023 ± 6.90 × 10–6
34 3.4 1696 0.000236702 ± 7.10 × 10–6
34 3.4 804 0.000215448 ± 6.46 × 10–6
34 1.6 804 0.000205581 ± 6.17 × 10–6
40 2.5 1250 0.000258393 ± 7.75 × 10–6