Defects in Metal Additive Manufacturing: Formation, Process Parameters, Postprocessing, Challenges, Economic Aspects, and Future Research Directions

R Haribaskar 1, T Sampath Kumar 1,✉
PMCID: PMC11443127  PMID: 39360135

Abstract

Metal additive manufacturing (AM) is a revolutionary technological advancement that has made significant inroads in a wide range of sectors, including aerospace, defense, automotive, health care, and engineering applications. It offers unprecedented design freedom, reduced material waste, and enhanced performance, in addition to significant enhancements to fabrication processes. Microstructural defects and internal stresses formed during fabrication directly affect the fabricated product's surface integrity, quality, and service life. Identification, characterization, and prediction of these defects help significant and direct production of defect-free structures with high density. This article provides detailed insights concerning the common defects, mitigation techniques, and challenges reported in both powder bed fusion-based and wire arc AM methods. Defects such as porosity may develop due to the powder sphericity, roughness of the powder, preheating, process parameters, build environment, postprocessing techniques, and environmental factors. Therefore, a critical study of the techniques, alloys, process parameter optimization, and different postprocessing techniques to tone down the defects is made from their formations.

Keywords: additive manufacturing, defect formation, process parameters, postprocessing, defect mitigation

Introduction

Additive Manufacturing (AM) process involves fabrication of three-dimensional objects or models through fusing or melting of the material layer by layer.1 AM evolves in a global way in the fabrication of complex models or structures on different materials, including stainless steel (SS), titanium alloys, nickel-based alloys, tool steel, aluminum alloys, and magnesium alloy, for different applications, including aerospace, automobile, biomedical, health care, implants, not getting fabricated using subtractive manufacturing or other forming methods, detailed in Table 1.2–7 AM techniques are widely dispersed in the fabrication of different polymers, ceramics, resins, and metal alloys.8–10 Binder jetting (BJT), directed energy deposition (DED), material extrusion (MEX), material jetting (MJT), powder bed fusion (PBF), sheet lamination (SHL), and vat photopolymerization (VPP) are the seven processes that compose ISO/ASTM 52900:2021(E), which classifies AM.11

Table 1.

Properties and Applications of Various Alloys

Material Properties Applications
Nickel alloys High strength, corrosion resistance, high temperature resistance Aerospace: Jet engine components, airframe structures, turbine blades, and exhaust systems. Chemical processing: Pressure vessels, and piping systems: marine; Power generation: Heat exchangers, steam generators, and turbine components. Nuclear: valves, fuel rods, and control rods
Aluminum alloys Lightweight, high strength-to-weight ratio, corrosion resistance Aerospace: Aircraft fuselages, engine components, wing structures, landing gears wing spars, skin panels, and stringers Automotive: Engine blocks, cylinder heads, transmission cases, and suspension components; complex geometries, heat exchangers, fuel systems
Steel alloys High strength, durability, low cost Construction, Automotive: Frames, body panels, and suspension components. Industrial machinery: Gears and shafts. Medical instruments: Surgical instruments, prosthetics, and orthodontic appliances. Defense: Tanks, armored vehicles, and weapons. Medical: Bone implants, prosthetics
Titanium alloys Strong, lightweight, corrosion resistance Aerospace: Engine components, stringers. Medical: hip and knee replacements, spinal rods, and dental implants. Automotive: Exhaust systems, engine components, and suspension systems
Magnesium alloys Lightweight, high strength-to-weight ratio, excellent machinability, excellent damping capacity Aerospace: fuselages, engine components, Automotive: steering wheels, steering column brackets, and instrument panel supports: Electronics; Biomedical: bone implants and drug delivery systems
Cobalt alloys High strength, high temperature resistance, biocompatible Medical: orthopedic implants, dental implants
Copper alloys High thermal and electrical conductivity, Good corrosion resistance, high strength Electrical wiring, electronics, heat exchangers, engineering components
Tungsten alloys High density, high melting point, high hardness Aerospace; defense; industrial, medical, radiation shielding, and electrical applications

PBF is a widely used technique in both research and industrial purposes, owing to its notable advantages such as accuracy, dimensional stability, and the ability to reuse the powder. PBF is the metal AM process that utilizes the laser heat source by melting the gas-atomized powder particles based on their powder particle distribution, which recognizing the layer thickness is then layered by the recoater after each layer of melting to fabricate the models.3,12 Also, the PBF process has some deficiencies that prime the defects through process parameters, laser parameters, preprocessing, postprocessing and environmental factors, which lead to the defects in building the specimen on the surface, subsurface, and lowering the mechanical properties such as microhardness, fatigue, tensile strength, and microstructural changes on fabricating the complicated models, meta-models, and lattice structure with thin struts.13,14

Metallic filler wire-based AM is another type of AM, in which a metallic filler wire is used to fabricate the product. The process is also commonly known as wire arc additive manufacturing (WAAM). In this method, an electric arc is used to melt the filler wire, which is then deposited onto a substrate to create a layer of the object.15,16 The process is repeated to build up the object layer by layer. The filler wire can be made of various metals, including steel, aluminum, titanium, and nickel-based alloys.17,18 WAAM has advantages over other AM methods, such as high deposition rates, the ability to use a wide range of metal alloys, and the ability to create large-scale objects.19–21

However, it also has some limitations, such as the need for an operator with skill and experience to obtain optimal results, the potential for high levels of distortion, and the need for postprocessing to achieve the desired surface finish in the AM processes (PBF, DED, etc.).22,23

Defects such as porosity, lack of fusion (LoF), uneven surface roughness and finish, balling, and residual stress (RS) drop the mechanical properties in the end product.24–26 In addition, controllable porosity in additively manufactured specimens provides benefits depending on the application, including lightweight structures in the automotive and aerospace industries, thermal management in airflow and cooling ducts, acoustic and vibration damping to absorb or control noise and vibrations in various applications, including automotive exhaust systems, mufflers, or architectural elements, and biological applications in the biomedical and tissue engineering fields. However, uncontrolled porosity can negatively affect mechanical properties and compromise the structural integrity of a component, which may result in a reduction in mechanical properties, whereas condensate scattering occurs at a higher volumetric energy density (VED). The dispersed powder material vaporizes, leaving porosity behind.

The keyhole phenomenon is another way material vaporization might trap gas in the melt pool. As a result of vaporization, scattering and porosity occur, when the powdered substance contains elements with a relatively low melting point. Research work has demonstrated the occurrence of lower the porosity (about <2 vol.%), lower the chance of component failure due to porosity during loading.27,28 According to the studies, the thermal gradient formed by the rapid heating beneath the laser beam contrasted with the moderate heat conduction found in AM materials and localized compressive and tensile stresses are generated, which leads to RS.

There is a significant temperature difference from the bottom to the top layer during the PBF AM process. The temperature gradient from the bottom to the top layer can cause uneven cooling and solidification rates, which can lead to undesirable outcomes, including nonuniform cooling, the formation of RS and warping, variation in the microstructure, inconsistent material properties, and delamination. In most cases, RS results in undesirable outcomes such as component distortion, reduced strength, and surface crack propagation. While the top layer is being heated, the bottom layer is already excellent, generating internal tensions in the sample. As a result, a stress relief (SR) heat treatment (HT) process and postprocessing techniques, including peening procedures such as laser shock peening, shot peening, hot isostatic pressing (HIP), lapping, and buffing, were preferred for the elimination of internal stress.29–31

RS was seen becoming more homogeneous within the component after a suitable postprocessing technique or SR HT, indicating reduced proneness of the component to failure due to RS seen during servicing.32–35 Surface flaws, such as surface roughness and surface quality, are a significant challenge in metal AM. Factors include decreased operational reliability and unacceptable poor surface finish conditions. Steep troughs on the near-surface favor location for mechanical destruction under loading and corrosion are especially damaging to the performance of the component.36–40 In metal AM, the high surface roughness can be a result of the high RS caused by unoptimized process parameters, which leads to warping and distortion, cracking, and delamination and can propagate along the surface, leading to irregularities on the surface and resulting in higher surface roughness. For example, high surface roughness can lead to a decrease in strength and ductility.

On the contrary, postprocessing techniques such as HT and surface finishing can improve the surface roughness and mechanical properties of the fabricated product. However, Figure 1 depicts the formation of defects and ensures the quality of the part by illustrating many influential factors in the cause-and-effect diagram.

FIG. 1.

FIG. 1.

Cause and effect diagram for the formation of defects.

This article provides a comprehensive review of the primary defects seen in the PBF-based, WAAM, and other AM finite element modeling, focusing on their origins and their effects on the fabrication phase. In addition, optimization, improvisation, constraints, efficient approaches, and postprocessing procedures for defect reduction are reviewed in each section. Finally, the future scope, economic aspects in defect reduction, recommendations, and difficulties in mitigating defects are discussed in detail.

Primary Defects in PBF Process

In AM processes, there will be three major categories of imperfections during fabrication at each stage. Also, during the stage of powder particle dispensing, irregularities develop on the powder bed. Additional defects and difficulties, including such powder spattering, may arise in nonsteady-state conditions. Identifying and mitigating defects are a crucial feature of metal AM toward enhancing the quality and efficiency of end products. Regarding each of these concerns, the defect development mechanisms involved are described below. This section discusses widespread development and prevention with each type of defect formation.

Porosity

The level of solidity achieved in an additively manufactured metal sample, when there are cavities or holes between the layers of the part, is called porosity. Whereas voids or cavities are classified into various forms during fabrication, such as gas porosity, which occurs during fabrication with the incorporation of gas pockets into the material and appears as small spherical voids, and shrinkage porosity, which is formed during the cooling and solidification processes when the material undergoes volume contraction and appears as small spherical or elongated voids. LoF, keyhole porosity, and balling are additional types of porosities, which are discussed in the following sections. Internal porosities or voids in laser powder bed fusion (LPBF) can occur under two different states of inadequate and excessive heat input. The former scenario results in lack-of-fusion voids, whereas the latter results in keyhole-induced pores.

Figure 2 shows the formations of different kind of pores with respect to the preheating temperature. Tables 2 and 3 epitomized the formation and mitigation of porosity and keyhole porosity. Various studies on porosity in different alloys are discussed in detail.

FIG. 2.

FIG. 2.

Formations of different kinds of pores with respect to the preheating temperature.152

Table 2.

Porosity: Reasons for Defect Formation and Mitigation Techniques

Defect Fabricated process/processed material Reason for defect formation Measures to minimize defect percentage References
Porosity DMLS/titanium alloy Rapid solidification, unmelted powder particles, gas entrapment due to higher scan velocity and higher laser power Reducing the power and scan velocity of the laser source 155
LENS/stainless Steel Porous powder particles Laser remelting 156
LENS/Inconel 718 Unoptimized process parameters Ultrasonic vibration-induced acoustic streaming and cavitation technique 157
DMLS/SS316L and titanium alloy Unmelted powder particles, oxidation, vaporization of unmelted powder, inadequate power deposition Essential to minimize discrepancies in layer thickness, laser spot depth, track width, and hatch distance. 158,159
Laser spot welding/analysis with COMSOL Oxidation, over melting of powder particles, vaporization due to lower melting temperature Maintaining the build chamber with minimal oxygen content, optimized laser power to fuse the powder particles 28,160
DMLS/theoretical guidance Improper hatching and interaction with the interlayer Mitigation of interlayer interaction by proper process parameters and optimizing the hatch distance 161

DMLS, direct metal laser sintering; LENS, Laser Engineered Net Shaping; SS, stainless steel.

Table 3.

Keyhole Porosity: Reasons for Defect Formation and Mitigation Techniques

Defect Fabricated process/processed material Reason for defect formation Measures to minimize defect percentage References
Keyhole porosity DMLS/TI6Al4V and SS316L High energy density with lower scan velocity, advancing laser-material interaction Optimization of process parameters 162,163
Laser welding/Al alloys Increased transient fluctuations, lower scan. or weld velocity Increasing the scan velocity, constant energy density 164
Laser fusion welding/titanium alloy Deposition of excessive energy to fuse the particles and cavitation Avoiding the oxidation state and minimization of laser power source 165
DMLS/Inconel625 Higher VED on the melt pool Attenuation of laser power source 166

VED, volumetric energy density.

Steel alloys

Ahmed Obeidi et al.41 investigated using the same processing parameters and SS316L material the mechanical properties and porosity of four PBF machines, including Aconity MINI, ProX200, EOSM280, and Cusing by concept laser that were evaluated. There were differences in the mechanical properties, density, porosity, and microstructure of all the four components fabricated with different machines. For example, ProX200 was used to increase the brittleness of the printed sample. In contrast, EOSM280 plays a crucial role in stabilizing the measured performance values and providing a stable austenitic structure. Cusing exhibits a lesser tensile strength than the other machines, while Aconity MINI and EOSM280 feature greater relative density. It was observed that the process parameters and built-in features of each machine play a significant role in optimizing the printing of each element.

For the elimination of material defects in the future, it is recommended to implement closed-loop control to optimize the process parameters according to the machine and material to be printed. Murphy-Leonard et al.42 tested the texture, porosity, and deformation of additively manufactured SS 316L using high-energy X-rays, where it underwent tensile loading. Behavioral changes were monitored using the X-ray computed microtomography (XCT) technique. The pore distribution was seen mainly on the surface of the sample, causing strain accumulation and the development of crack growth by uneven pore distribution during tensile loading. According to Ball et al.,43 the scan speed and porosity of the SS 304L LPBF samples were evaluated using the two-point correlation function.

Statistical analysis of porosity in 304L LPBF samples was made through changes in the scanning speed from 50 to 700 mm/s. Increasing material porosity was seen following an increase in the scanning speed of the laser. Tapia et al.44 evaluated porosity using the Archimedes' principle by printing the materials. Also, a new model was developed to analyze the porosity using the Kriging method. The Kriging model developed was based on the spatial Gaussian process, where evaluation of the porosity was done under varying laser power and laser scanning speed. 17-PH 4 steel was fabricated and taken for evaluation and validation of porosity with the help of two methods. Validation of both the methods resulted that the laser power of 50 W and laser scanning speed of 275 mm/s provide a lower porosity of 0.325%.

Nickel alloys

Panwisawas et al.45 made a study of the analytical framework of LPBF with the help of computational fluid dynamics modeling from solid–liquid–vapor transformation for obtaining the thermophysical properties, porosity, and cooling rate of nickel-based superalloys. The rate of porosity is higher when the thermal conductivity of the material is low. This is due to the presence of voids disrupting the flow of heat, which lowers the total contact area between solid parts of the material. Also, volatile mass loss and porosity are lower when the thermal conductivity is higher in the high viscosity region. A high rate of cooling leads to significant RS formation. Optimization of process parameters is suggested at the stage of manufacturability for ensuring a good-quality product.

Babamiri et al.46 evaluated the microstructure and mechanical properties of additively manufactured Inconel 718 related to as-built, stress relieved at 1065.5°C for 1.5 h on vacuum environment and HIP with temperature of 1163°C, and pressure of 102 MPa for 4 h. At every HT process, the porosity sloped down to a reduction of about 97% due to void closure and 50% enhancement of yield strength due to the recrystallization and formation of annealing twins.

Titanium alloys

Xiong et al.47 developed a functionally graded porous structure for reduction in porosity defects in Ti-6Al-4V, where porosity affects the mechanical properties with prospects of enhancement. A functionally graded porous structure was developed with different stacked conditions and is evaluated using finite element analysis (FEA). The metal sample tested with compression showed improvement. Also, the developed functionally graded porous structure led to improvement in elastic modulus and yield strength. Defects and porosity are eventually scattered, whereas the denser region showed limited flaws. Muro-Barrios et al.48 identified defects such as crack growth, porosity, and dislocation as standard in 3D ductile fracture models of metal AM, which are influenced by many process parameters such as laser power, orientation, scanning speed, and hatch distance.

Porosity was figured to have a greater impact on the metal sample, causing crack growth and larger defects with premature failure. However, crack growth occurred in the horizontally built samples with the help of void clusters in the same plane, whereas void clusters resulted in crack-tip blunting in the vertically built samples.

Liu et al.49 measured the porosity of the DED samples using transient thermoreflectance. The algorithm developed was meant to finding the porosity using thermoreflectance metadata retrieved from the source. Four different samples were printed with different laser output and printing schemes such as two-layered planes, three two-layered planes, and no deposition form. Porosity of the printed sample was determined and comparison was made with the outcome of the developed algorithm producing the same result. Pappas and Dong50 saw an increase in the density of additively manufactured transparent MgAl2O4 sample when the scan speed was increased up to 2000 mm/min. A drop occurred with more incredible scan speeds. The extended melt time in conjunction with the higher laser output and the temperature caused a reduction in the ceramics.

Lifton and Liu51 evaluated porosity in additively manufactured samples using the XCT technique. However, ultimate results were not seen due to the lag of processed and scan data. The missing and processing data were incorporated with the algorithm developed using Python by referring to the literature relating to defects in the porosity of the metal additive samples by comparing the XCT values, as shown in Figure 3. The algorithm helped in the production of reliable results compared with the XCT values. Vargas-Uscategui et al.52 optimized the trajectory path of the nozzle using the robotic simulation for a reduction in porosity of the sample and evaluation using cold spray additively manufacturing. The preprocessed toolpath showed higher porosity that misguided the material.

FIG. 3.

FIG. 3.

XCT images showing porosity in percentage (a) 0.2, (b) 1.4, (c) 3.51 XCT, X-ray computed microtomography.

Therefore, the toolpath strategy was modified from square to round hump for the guidance to porosity reduction where the pore distribution was higher in the edge and smaller in the interlayer and in the intertrack region. This enabled production of the best near net shape. Hamid et al.53 developed a dog bone-shaped model for analysis of viscoplasticity, dislocations, grain refinement, and structure. Evaluation of additively manufactured structures was done with the stress–strain viscoplasticity model using LS-DYNA, and the dislocations were examined. Grain refinement was seen with more significant effects on the structure than softening caused by porosity according to the developed model. Khalil et al.54 evaluated failure caused by variations in porosity in the additively manufactured samples.

Deterioration seen in the microstructure of the metal additive samples to an imperfect level made it mandatory to quantify the failure, process parameters, porosity, and plasticity. Therefore, techniques were developed for quantification of the same pseudomarginal and embedded variability, A computed tomography (CT) scan was evolved for the evaluation of the porosity level. Ning et al.55 evolved the analytical and physical models for a reduction of porosity for evaluation of the system. A systematic approach to finding the porosity was made using the evolving front approach and investigation of the image. Investigation was done with the melt pool dimensions and thermal analysis of the system. Finally, the calculated front approach porosity was determined and validated by the mechanical values calculated using different techniques stated in the literature.

The preceding section provided a description of the effect of porosity on metal additive-manufactured samples of various materials in detail. Higher scanning rate, lower laser power, lower thermal conductivity, toolpath strategy, grain refinement, and laser scattering increase porosity, reduces the mechanical properties such as tensile, fatigue, and microhardness. There was a drop in the fracture rate and fatigue life when the pore size exceeded 85 μm. Optimization of the process parameters under the material and machine interaction, round hump scanning strategy, grain refinement by optimizing the process parameters and postprocessing, pulsed alternating current (AC) mode for laser, cold spray additive technique, and functionally graded porous structure helped in reducing the porosity of additively manufactured samples.

Lack of fusion

LoF is the subset of the defect called porosity, which typically arises due to various factors such as inadequate energy input, improper laser parameters, insufficient powder bed preheating, or an incorrect scanning strategy during fabrication. Powder particles may not completely melt or fuse together as a result of these factors, causing gaps or weak interfaces between layers. The formation of LoF is shown in Figures 4 and 5. Table 4 epitomized the formation and mitigation of LoF and this section deals with the LoF formation in depth of different alloys.

FIG. 4.

FIG. 4.

Hydrogen-induced LoF and keyhole pore formation.153 LoF, lack of fusion.

FIG. 5.

FIG. 5.

Oxide layer pertained LoF formation.153

Table 4.

Lack of Fusion: Reasons for Defect Formation and Mitigation Techniques

Defect Fabricated process/processed material Reason for defect formation Measures to minimize defect percentage References
Lack of fusion DMLS/analysis of all materials In stabilization of melt pool, Incompletion of particle melting Laser power source and laser parameters Optimization 25
Poor heat dissipation Calibrating the process parameters by fabricating the perfect thin geometries
DMLS and EBM/Inconel625 Retainment of unmelted powder particles due to insufficient heat input Providence of suitable laser power and hatch spacing 167

EBM, electron beam melting.

Steel alloys

Laleh et al.56 had insights into the LoF in powder bed-fused 316L SS. The coupons were made with a layer thickness of 30 μm, laser power ranges from 125 to 175 W, scanning speed ranges from 400 and 800 mm/s, hatch spacing ranges from 80 and 120 μm, and exhibits to the micro-CT. Recrystallization areas were seen while using electron backscatter diffraction around the spatter-LoF structures. Spatter-LoF structures were produced due to the voids, oxide layer, dislocation, and grain modification, and the formation of spatter-LoF is shown in Figure 6. Ronneberg et al.57 examined the relationship between the LoF, porosity, HT, and microstructure in additively printed SS316L in the cylindrical sample. The samples were placed in a furnace for 1 h at different temperatures of 700°C, 800°C, 900°C, 1040°C, and 1200°C, and allowed to cool to room temperature. Higher pores seen in the LoF region caused failure in ductility.

FIG. 6.

FIG. 6.

Formation of spatter-LoF.154

The horizontally built sample showed a major significance in porosity and ductility compared with the vertically built sample. The HT made a significant improvement in the mechanical properties and grain refinement enhancement. Bruna-Rosso et al.58 validated the LoF porosity using numerical investigation based on experimental data provided in the literature on SS316L and evaluated the model using a high-speed imaging camera. The Goldak heat source model was identified for evaluation by defining selective laser melting (SLM) parameters and geometric dimensions. LoF occurred in the first tracklayer due to the insufficient heat input for melting the excessive amount of material in the melt pool. This model enhanced productivity by optimizing the process parameters before fabricating the samples.

Nickel alloys

Shrestha and Chou59 fabricated samples using Inconel 625 powder using the PBF technique for evaluation of an LoF pore, and keyhole pores using the micro-CT technique. Nine samples were fabricated with different process parameters combined with VED. Keyhole pores were formed at a higher VED inside the pathways, and LoF pores at a lower VED between the laser pathways. In contrast, there was an increase in the average pore count at a higher and lower VED compared with the nominal VED (81.25, 54.17 J/mm3). dos Santos Paes et al.60 made a study of the LoF of two different materials, Inconel 625 and iron, fabricated using the PBF technique. First, the void level for the samples was evaluated using ImageJ software and MATLAB code, and then the samples were subjected to remelting for getting a higher density.

Both the samples were remelted using an ytterbium fiber laser at different energy densities of 31.5, 38.2, and 45 kJ/m. Following the remelting process, the void percentage of iron sloped down to 1.7% from 5.3% to 7.1% at 45 kJ/m. On the contrary, the void percentage of Inconel 625 slopes down to 3.7% from the range of 4.4% to 7.1% at 31.5 kJ/m. Therefore, the void level reduction was not seen as significant in repeatability for Inconel 625, whereas for iron, it was significant.

Titanium alloys

Promoppatum et al.61 worked on the LoF on additively printed Ti6Al4V using a constant laser diameter of 100 μm, a layer thickness of 30 μm, scanning speed, energy density, and scanning rotation. LoF was assessed mathematically through use of the geometric method and three different techniques, namely, Archimedes, micrograph-based, and micro-CT. The analytical model results showed that the influence of melt pool dimensions is due to the layer thickness of the powder. The micrograph method was identified as most effective for identification of LoF and porosity. The sample fabricated with 66.7 J/mm3 of VED, 67° of scanning rotation, 750 mm/s of scanning speed, and 150 W of laser power showed a lower porosity of 0.0001 in micrograph-based evaluation.

Bustillos et al.62 analyzed the LoF in additively printed Ti Grade 5 alloy were printed as fully denser and fabricated the LoF samples by altering the process parameters. The laser power and scanning speed for a fully denser sample were 300 W and 700 mm/s. The LoF samples were printed with 100 W and 1300 mm/s with a constant scanning rotation of 67°. Under two conditions, the samples were exposed to HIP: 900°C for 2 h and 1000 °C for 1 h, and attained the micrograph-based porosity test using ImageJ software. The HIP exhibited the duplex microstructure in both denser and LoF samples, reducing defects on LoF sample and enhancing tensile and ductility. The LoF in the additive samples was controlled using optimized energy density.

Coeck et al.63 predicted the LoF pores in Ti6Al4V using the data compiled from micro-CT and data tracking of laser using data acquisition (DAQ) system incorporated into SLM machine for prediction of LoF pore before or while printing the samples. The data from micro-CT and DAQ process signals showed a correlation by about 90%. The predictive result on the range of LoF pores was in the diameter of 160 μm and volume >0.001 mm.3

Cobalt chromium molybdenum alloys

Darvish et al.64 fabricated CoCrMo coupons by varying the laser power from 180 to 360 W at an increment of 20 W with a constant scanning speed of 700 mm/s, hatch spacing of 125 μm, and layer thickness of 30 μm. When the laser output was increased to 260 W, the penetration depth was negligible, when compared with 240 W coupon. Track size and stability of the laser increase with increasing the laser output. LoF developed due to the irregular track and insufficient track size, inadequate overlapping percentage, and overlaying distance.

Mukherjee and DebRoy65 quantified to minimize the LoF based on the numerical analysis of transient heat transfer and fluid flow to derive the dimensionless calculations, the temperature, and pool dimensions. Using constant process parameters, numerical analysis and experimental validation were done through the comparison between three different materials, SS316, Ti6Al4V, and 10Mg, for three layers with five hatches. A higher laser output with lower scanning speed or performing both can provide a larger liquid pool and reduce the possibility of an LoF defect. The least but most susceptible to the LoF were 10Mg and SS 316 on printing with the same process parameters when compared with the Ti6Al4V alloy.

Tang et al.66 developed a geometry-based model with Rosenthal equation for the analysis of void-based LoF caused by unfused material. The model included material data under different conditions presented in literature. The analyzed and literature data matched with higher significance, forecasting the LoF, and porosity develops with the process parameters, layer thickness, hatch spacing, and laser scanning speed.

The section discusses the influence of process parameters and other factors contributing to the LoF. The keyhole and LoF pores are developed at a greater and lower VED, whereas the average pore count increases with higher and lower VED. The LoF induces spatter due to the impact of voids, oxide layers on the build chamber and material, dislocation, unstable grain refinement, uneven laser track, insufficient overlapping percentage, and overlapping distance. The LoF was minimized through optimization of the process parameters, a higher laser output with a lower scanning rate, optimized VED, grain refinement by postprocessing techniques, and remelting of the layer, which reduces LoF and improves the layer's density and mechanical properties.

Balling

Balling effect, also known as balling up or bead up, generally arises as an unfavorable defect in the PBF process, a complex metallurgical process and a foundation for mitigating porosity. Wetting exertion between the liquid–metal interaction and the solid surface, an uninvited outcome may cause a rise in breaking up the liquid scan track in PBF, resulting in molten globules against a smooth unvarying solid surface and creating particles in spherical shapes. Table 5 epitomized the formation and mitigation of balling and this section deals with the balling formation in depth of different alloys. Figure 7 represents the mechanism of balling formation.

Table 5.

Balling or Bead Up: Reasons for Defect Formation and Mitigation Techniques

Defect Fabricated process/processed material Reason for defect formation Measures to minimize defect percentage References
Balling DMLS/Inconel 718 Irregular size of powder particles, higher size of powder particles exceeds the laser spot diameter, uneven spread by recoater Powder size and sphericity, shielding gas optimization 75
DMLS/Ti-40Al-9V-0.5Y and titanium alloy Uneven laser scanning interval and unoptimized laser parameters, interruption in solidification due to larger particle size Scanning speed and laser power optimization 68,70,168
DMLS/SS316L Higher VED with higher laser power and lower scanning speed produces the deep thermal gradient on the melt pool Attenuation of VED and laser power 169
DMLS/Ti-6Al-4V Viscosity and surface tension of the melt pool become high due to lower volumetric energy deposition Utilization of optimized volumetric energy deposition 69
Iron-based powder Surface tension typically attempts to spheriodize the liquid, prevents the liquid metal from wetting the substrate Lowering the surface tension of the molten liquid 32

FIG. 7.

FIG. 7.

Mechanism of balling formation.69 (a) Scanning with low ED and small ball formation. (b) Mixing of materials with small balls. (c) Remelting of the same layer and laser reflection. (d) Balling effect due to remelting. (e) SEM image of a side surface, along with balling effect by rescanning of the layers. (f) A crack on the surface of a ball surface. ED, energy density; SEM, scanning electron microscope.

Steel alloys

Liu et al.67 investigated the microstructural and mechanical behavior of American Iron and Steel Institute (AISI) 420 SS with a 5 wt. % TiC content. The sample micrograph optimized had a greater energy density, resulting in an even distribution of TiC and a quick cooling rate. The densification behavior was determined independently by laser power and scanning rate. As scanning speed increased, the relative density of the sample gradually decreased, but the relative density increased with increasing laser power. Whereas the densification behavior reduced as a result of a short laser exposure and insufficient energy input. Furthermore, when exposed to surface tension, the molten metal shrinks into spheres (the bead up), owing to inadequate energy contribution, leading to a greater melt viscosity and a reduction in overall mechanical properties.

Gusarov et al.68 used the Plateau–Rayleigh capillary instability equation in the analysis of the stability and model the heat transmission in SLM. A single-track study was performed on selective laser melted SS316L, in which the laser heat was transmitted from the melt pool to the powder in the build substrate and flowed with surface tension. The length and the diameter of the melt pool expanded when the scanning speed or velocity dropped.

Titanium alloys

Pal et al.69 examined the top, bottom, and lateral surfaces through variations in the process parameters and rescanning a layer in Ti6Al4V alloy on SLM. Microcracks in the vertical direction initiated were due to lack of laser power, scanning velocity at a lower level, and incompletely melted powder particles. The surface morphology of the sample was seen as primes by the melt pool cooling time and viscosity. Compared with the process parameters used in the fabrication of a rough surface, rescanning the layer achieves the smoothest surface through remelting of the roughest surface. Rescanning surface built had a higher energy density and laser power, lower scanning speed, and the same overlapping laser track.

Gao et al.70 fabricated the Ti-40Al-9V-0.5Y alloy for inspection of the effect of process parameters on constructing the single track using SLM. When all other parameters were held constant, the balling effect developed on single tracks with an increase in the scanning velocity. There was expansion in laser focus breadth with a rise in the defocusing distance, but the depth and aspect ratio dropped. The thickness of the layer seemed to have no impact on the breadth, depth, or aspect ratio, but with a warm relationship with the contact angle. The laser volume energy density decreased with increase in scanning velocity, defocusing range, and layer thickness, increasing single-track cracking sensitivity. In contrast, cracks were eliminated through increase in the laser volume energy density by improving SLM process parameters.

Magnesium alloys

Liu and Guo71 obtained the balling effect in magnesium AZ61 alloy through variations in the scanning speed from 250 to 950 mm/s, with an interlude of 50 mm/s. There was a decrease in laser energy density with a rise in scanning speed of the laser track, causing deterioration in the balling effect. This negative consequence caused a shortage of energy primes, followed by a rise in viscosity and surface tension, resulting in uneven liquid flow. The sample had a relative density of 99.4% due to the laser track's 300 mm/s scanning speed and 156.2 J/mm3 laser energy density. Dispersion and densification of magnesium particles happened simultaneously, interacting with each other, as shown in Figure 8.

FIG. 8.

FIG. 8.

Balling effect at different scan speeds of magnesium alloy.71 SEM images of AZ61 magnesium alloy under different scanning speeds: (a) 950 mm/s, (b) 900 mm/s, (c) 850 mm/s, (d) 800 mm/s, (e) 750 mm/s, (f) 700 mm/s, (g) 650 mm/s, (h) 600 mm/s, (i) 550 mm/s, (j) 500 mm/s, (k) 450 mm/s, (l) 400 mm/s, (m) 350 mm/s, (n) 300 mm/s, and (o) 250 mm/s. Black arrows used for the indication of Balling, Pores and unmelted powder as mentioned in the figure. Black dotted lines represents the visible scan track.

Tungsten

Zhou et al.72 studied the balling effect in powder bed-fused tungsten through variation in the laser exposure time to 200, 300, and 400 μs on the surface and rescanning the surface layer. The balling effect related to the laser exposure time resulting in the discontinuous beads. Drops with W-shaped distribution were formed at 200 μs, whereas a closely packed bead structure was formed at 300 and 400 μs. The double exposure time of 200 μs as closely packed balling beads with pores and debris filled with W-shaped distribution. The best laser exposure time of 300 μs to rescan the surface resulted in a defect-free smoother surface with a density of 15.2 g/cm3 on the first scan, and 16 g/cm3 on the second laser scan helping in getting a defect-free surface.

Li et al.73 investigated the balling effect in SLM of SS and Ni powder through variations in the layer thickness, laser power, surface remelting, scanning speed, and interval. The balling effects categorized with 500 μm ellipsoidal beads and 10 μm spherical beads increased the surface roughness. Both SS and Ti powders show the same results. In contrast, a surface with no beads and pores was produced by a greater laser energy density, lower laser scanning speed, lower oxygen content in the constructed chamber, single remelting track with no scanning interval, and overlapping. Yadroitsev et al.74 evaluated and analyzed the formation of a single track with the process parameter scanning speed and power of the laser at a lower level in different materials such as SS316L, SS904L, Tool steel H13, Inconel 625, and Cu alloy.

The balling has occurred among these powder materials of SLM on Cu alloy single track built with 0.15 m/s scanning speed, where the irregular formation of balling beads in the build platform was seen when the scanning speed was at a lower and significantly higher level. The scanning speed was higher for higher laser power for the material with higher thermal conductivity. Kruth et al.32 used iron-based powder with a combination of Fe, Ni, Cu, and Fe3P for processing with SLM. The process parameters were optimized and adjusted for fabrication and evolved for mechanical and microstructural characterization for elimination of significant defects. Highly dense parts with no balling effects were achieved using 300 W laser power for fabrication. The higher bending capability occurred with the higher density sample of 91%.

Ladewig et al.75 looked at the effect of shielding gas on SLM product quality. Guidance to the shielding gas in a homogeneous flow with a constant flow speed or velocity covering the surface without interacting with the laser helped elimination of the by-products of SLM with shielding gas interactions. There was a reduction in VED, when a laser scattered due to shielding gas, resulting in insufficient heat or energy to fuse the powder, resulted in a spherical bead known as the balling, as a significant cause for LoF failure.

Analysis of balling was seen as the leading cause of porosity. Lower VED or lower laser power with higher scanning speed, laser exposure time, shielding gas, laser scattering, and insufficient energy level with scanning speed induced surface tension liquid flow, which in turn caused shrinkage in the molten metal. The bead-up was reduced through optimization of the process parameters, rescanning the built layer with a higher VED, overlapping laser tracks and an overlay region, and reducing the oxygen content in the build chamber with no scanning interval, which resulted in a surface with fewer defects and a more robust component.

Residual stress

The term “residual stress” refers to the internal or mechanical stress that forms in metal additively manufactured parts due to repetitive heating and slow cooling during the PBF process. Stress induced beyond the elastic limit in metal parts occurs due to rapid cooling on the smaller volume of a higher temperature gradient, where plastic strain is generated during the heating cycle, restricting material shrinkage, resulting in tensile RS in the earlier agitated region of the selective laser melted part that leads to the deformation, warpage, dimensional instability, increased corrosion rate, and stress corrosion cracking. Table 6 epitomized the formation and mitigation of RS and this section details the study of RS on various metal alloys.

Table 6.

Residual Stress: Reasons for Defect Formation and Mitigation Techniques

Defect Fabricated process/processed material Reason for defect formation Measures to minimize defect percentage References
Residual stress Residual stress/MAM-Review Higher energy density, rapid heating to cooling cycle Attenuation of energy density 170
DMLS/CoCrFeMnNi
Alloy
Higher laser power needed to fuse the high entropy alloy produces leads to the formation Reduction with the help of cryogenic treatment 96
DMLS/AlSi10Mg Rapid and repetitive heating to cooling cycle Deep cryogenic treatment reduces 73% of residual stress 96
DMLS/SS316L Incompatibility of thermal gradients between the fabricated layers Optimization of laser process parameters 34

MAM, Metal Additive Manufacturing.

Steel alloys

Kumaran et al.76 fabricated a DED sandwich structure over the PBF substrate and examined the RS on the heat-affected and interface region of SS316L. The interface region had a lower and more beneficial compressive RS of −889 MPa, while the DED and PBF regions had −707 and −552 MPa, respectively. Wu et al.77 developed an optimized segmented heat source (OSHS) model for enhancement of laser-based PBF numerical modeling precision and effectiveness. OSHS had the ability to minimize computation time by one-third compared with fine mesh and produces nearly a similar thermal–mechanical product. An SS 316L coupon was fabricated using PBF for the verification of the calculated results. The predominant surface RS sample was the tensile stress laterally on the scanning track of the laser, roughly 280 MPa, where the as-built sample corners had high shear stress.

Narvan et al.78 observed not only the elimination of fracture and cracks by preheating the base plate at 200°C, but also the elimination for stress relief postprocessing. The RS for sections with more than 97% relative densities was independent of the densification level, and also the preheating restricts the transformation from martensite phase. According to the results of deflection modeling, the martensite start temperature should be set as the relaxation temperature for steels undergoing martensitic-phase transformation. Williams et al.79 fabricated powder bed-fused 316L SS in the investigation of the result of postprocessing HT on RS. Immense tensile RS of around 450 MPa was projected at the outer gauge surfaces of the vertical angle. The horizontal sample had substantially lower RS by roughly 40%.

Nickel alloys

Pant et al.80 used neutron diffraction for mapping RS on additively manufactured Inconel 718 with optimized process parameters through variations in the build orientations as vertical, horizontal, and 45° inclination. The experimental results were consistent with the simulated results, with RS being higher in vertical built, slightly lower in 45° inclination built, and the lowest in horizontal built specimens, as shown in Figure 9. Preference of horizontal built to flat samples was seen, whereas vertical built and 45° inclination build were seen as preference to thin-walled structures. Watkins et al.81 analyzed the neutron diffraction technique in their investigation of RS in Inconel 718 manufactured using SLM with variation in the process parameters. RS distribution in the subsurface range was tensile, but as the depth increased, the distribution became compressive. The processing parameter energy density had no effect on RS, whereas increasing the energy density had a direct effect on grain refinement.

FIG. 9.

FIG. 9.

Comparison of experimental and FEM results for build direction of 45° sample at cross sections.80 FEM, finite element method.

Goel et al.82 evaluated RS in nickel-based superalloy Alloy 718, and neutron diffraction was used in the evaluation of RS in PBFs created with electron and laser energy sources. Thermal post-treatments efficiently minimized the RS of the material or self-equilibrating stress. In the case of laser-based PBF, the checkerboard method had the lowest level of RS due to the homogenous heating when analogized toward a bidirectional raster scan pattern. Nadammal et al.83 examined the effects of four distinct scan techniques in the formation of micrograph, texture, and RS with SLM Inconel 718. According to Von Mises equivalent stress charts, the alternating and rotational scan techniques have lower stress values and gradients.

Sirin and Kaynak84 evolved one of the most widely used and practical methods for predicting RS and distortion during AM, the finite element method (FEM). The simulation in this work used laser PBF of nickel-based superalloy (Inconel 718). In addition, the influence of laser scanning factors such as the power of the laser, scanning speed, layer thickness, and scanning technique was also examined. As a result, the chess part had the most considerable RS, which was visible on the surface of all sections. Furthermore, the power of the laser and scanning speed had a significant impact on the distortion angle. As a result, part deformation caused reduction in the usage of stress relief HT.

Wang and Chou85 studied the micrograph and self-equilibrating RS of Inconel 718 coupons in both as-fabricated and stress-relieved circumstances. Fine equiaxed and columnar cellular dendrites were visible in the transverse, frontal, and sagittal planes. Interdendritic zones and interlayers were seen having Laves phases. The homogeneity of the microstructure caused a reduction in the highest compressive RS from 378.4 to 321 MPa.

Titanium alloys

Emanuelli et al.86 utilized CT and XRD for the investigation of the impacts of internal defects and turning RS in selective layer-melted titanium alloy. The fatigue fracture initiation point was pushed below the outer surface by surface compressive RS, increasing the notched specimen fatigue strength. The total elongation and energy utilization were affected mainly by the heat-treatment temperature. Zhang et al.87 examined RS and density in the laser-based powder bed-fused titanium alloys by adjusting the energy density at 60 and 85 J/mm3 levels. Lower energy density produced lower RS with higher density, whereas higher energy density created higher RS with lower density and higher pores. The increased RS produced α’ orientations into the needle and stripe-like α’ phase, which primed the dislocation in the as-built sample. With twins, the lower VED resulted in lower tensile strength, while the higher VED resulted in higher tensile strength. The mechanical characteristics of the laser powder bed-fused titanium alloys had a significant influence from pores, RS, and microstructures. However, the intrinsic interactions among the self-equilibrium RS and the micrograph of the α’/α phase revealed the ability of twin deformation to produce significant improvement in the recital of the α’/α+β phase in laser powder bed-fused titanium alloys.88–92

Levkulich et al.93 used three distinct approaches in their study of the result of RS in the effect of process parameters fabricated using powder bed-fused titanium alloy: XRD, hole drilling, and contour technique. The initial RS condition can be crucial before LBPF for the growth of RS before LPBF.

Both the surface layer of substrates and deposition and the RS distribution of substrates and LPBF had an impact from by RS pattern throughout the deposit thickness and the processing parameters. Pauzon et al.94 evaluated that the residual surface stress with the use of XRD in the thin coupons (220 MPa) was much lower than in the cuboid coupons (645 MPa). The shorter laser vector length was seen as the cause for the difference resulting from the accumulation of heat and stress reduction. Robinson et al.95 determined the RS of powder bed-fused titanium powder through variations in the laser scan strategy. Samples were made using seven different laser scan strategies, including trajectories in the X and Y track, shifting scan vectors in X and Y directions, 2.5 mm checkerboard with 1 mm offset, 20 mm checkerboard with 1 mm offset, 5 mm checkerboard with 1 mm offset, and no offset.

Hole drilling neutron diffraction RS measurement provided a more accurate quantification than the contour method. In addition, the checkerboard scan strategy helped a slight reduction in RS. On the other hand, the changing X-Y scanning strategy distributed the stress uniformly throughout the solid and attained the lowest RS of all the scanning strategies.

Aluminum alloys

Zhou et al.96 show that utilization of the high-energy density occurrence on the melt pool throughout the manufacture of 10Mg alloy by laser PBF resulted in repeated heating and cooling, with RS. Deep cryogenic treatment (DCT) is a technique that involves subjecting the fabricated specimen to extremely low temperatures, typically around −196°C, for a duration of 24 h before stabilizing it to room temperature. This deep-freezing stage plays a crucial role in relieving RS and promoting grain refinement, both of which are inherent in the PBF process. The extreme cold temperature slows down atomic diffusion, resulting in the formation of finer grain structures, thereby enhancing the mechanical efficacy and stability of the material.

The results show that the DCT technique can release up to 72.7% of RS by using the strain-gauge hole-drilling technique. In addition, compared with heat-treated samples, tensile strength of the DCT samples increased by 245 MPa, with hardness in 56.72 HV increases.

Sunny et al.97 examined the effects of micrograph modeling and intrinsic RS mapping on the hybrid metal-additive process. Heterogenous laser powder bed-fused micrograph modeling presents in anisotropic plastic strain and RS on the burnished planar surface. Elevated temperature reduces the compressive RS through scan line and hatch spacing.

This section makes a comprehensive analysis of RS, forms with vertical build orientation, increased layer thickness, and unoptimized process parameters. The SLM method generates higher RS than the DED process, and the interface zone between the two processes (SLM-DED) produces superior compressive RS. The checkerboard scanning strategy, X-Y scanning strategies, and alternation in rotational scanning strategies generated a lower and more uniform RS distribution than any other scanning strategies. RS achieved was minimum for flat samples with horizontal build orientation. However, the vertical or 45° build orientation was preferred for thin-walled structures. The thermal postprocessing procedures, preheating the build platform, and the DCT approach minimized RS compared with the as-built condition.

Surface Roughness and Surface Finish

Surface roughness and finish are essential in engineering and biomedical applications involving metal AM, as rough surfaces provide higher stress concentrations, which can contribute to fracture initiation, increased wear and corrosion rate, and fatigue failure.98–100 Microvalleys and slopes, textures, irregularities, and pits in the surface and subsurface are measured by surface roughness. It remains challenging to obtain defect-free surfaces for additively manufactured metal components, and so, advances in process control, material development, and design practices continue to push the boundaries of improving surface quality in AM to minimize and control defects. This section deals with the surface roughness and finish of different alloys in depth.

Steel alloys

Shen et al.101 fabricated 316L SS samples using the PBF technique characterized in terms of morphology and roughness. Three powders that had not been sintered and two sintered areas were investigated. Surface material removal methods were investigated using experimental and modeling data. Unsintered powders on SLM surfaces dissolved faster during electropolishing due to microstructure variations. Pool borders degraded faster than protruding areas. Continuous electropolishing of sintered regions was seen to be possible with a longer electropolishing duration. The Ra and Rz values of polished surfaces decelerated from the beginning to the end of electropolishing. Rz is lowered from 10 to 20 min due to sintered area roughness.

Yang et al.102 made a study of 17-4PH SS manufactured with LPBF and examined the specimen surface quality. Optimization of AM parameters with the laser power ranging from 90 to 490 W and scanning speed 400–2200 mm/s with the VED ranges from 70 to 100 J/mm3. VED ranging from 70.31 to 97.66 J/mm3 and post-processing procedures provides high quality 17-4PH stainless steel as-built coupons with the relative density up to 7.70 g/cc. Typical surface roughness was 12.94–15.92 μm, suitable for use in practice. Low as-built density caused surface flaws. Automatic mechanical polishing improved sample surfaces. Fine finishing reduced surface roughness by 856% with polishing ranging from 200 to 2000 grit emery paper, followed by disc polishing. Physical vapor deposition coating improved shine by 188.9%.

Liang et al.103 used the computational techniques in the analysis of the individualistic and competing influence on the surface flaws and microstructural elements in an additively manufactured SS-316L. LoF flaws outweigh texture, roughness, grain size, and morphology. Preferred grain orientation on the fatigue behavior of SLM SS 316L is seen lowering the endurance limit by 10%. Without an LoF defect, the roughness assessed in the produced specimen had no discernible impact on fatigue strength. Blinn et al.104 observed the outcome based on the stress relief HT technique on SLM specimens. Differentiation between polished and additively produced surfaces was studied. HT decreased hardness and yield strength for both the building orientations. HT increased fatigue strength in horizontally built specimens. Postprocessing AISI 316L selectively laser-melted structures with stress-relief heat are advised.

As-printed samples revealed a dual-staged S-Nf curve in a high cycle fatigue regimen, driven through a transition since cyclic elastic deformation to microplastic deformation on higher stress levels. Wu et al.105 studied the effect of scanning pattern on the surface finish using magnetic field using SS-316L steel disk surface with varied orientations and scan techniques. SLM was seen having the ability to provide the correct net-shape geometry, but with as-built coupons having poor surface conditions. Magnetic abrasive finishing techniques can improve surface roughness and RS. Sarkar et al.106 studied the effect of SLM surface modification approaches. Electropolished LPBF-15–5 PH- SS improved fatigue life by ∼100%. According to fractography, surface roughness, subsurface flaws, and micronotches initiated cracks in SLM specimens. Laser surface remelting reduces surface roughness (91.2%) and subsurface flaws.

Electropolished surface roughness (Ra) was reduced by 97.4% compared with as-built. Iron and nickel dissolve preferentially, leaving a chromium-rich surface that increases corrosion resistance. Yamaguchi et al.107 focused on postprocessing SLM-made 316L steel components. Magnetic particle-based contact tool reduced the surface roughness Rz from over 100 mm to 0.1 mm. Tool manipulation along surface featured smoothes and removed fine material from the bulk area, though changing longer wavelength characteristics minimally. Portella et al.108 fabricated selective laser-melted 316L-SS samples and probes postprocessing. Post-processing technique called Surface Mechanical Attrition Treatment (SMAT), enhances the microhardness and surface quality by reducing the surface roughness. The partially melted powder particles on the surface of specimens produce a high level of roughness, which was significantly decreased by the SMAT postprocessing technique.

Nickel alloys

Detwiler et al.109 focused this research on Inconel 718 samples fabricated using SLM for estimation of as-built surfaces using processing parameters. The surface topography parameters computed with the use of a nine-point peak-evaluation technique had good agreement with the LPBF process parameters. With increase in layer thickness, enhancement of laser energy or decelerating down the scanning rate kept the VED constant. As a result, there was a rise in the up-facing as-built surface roughness and a reduction in the down-facing surface roughness for samples with a built-orientation of 60°. In addition, partially fused powder particles can be found on down-facing, as-built, near-surface regions, while a staircase effect can be found on up-facing surfaces.

Kumar Maurya and Kumar110 examined the impact of building orientation and HT on an additively fabricated IN718 alloy. The samples built with 45° built orientation provided lower surface roughness, but 90° built samples and HTs had no meaningful effect. Homogenization holding time had an effect on micrographs, precipitates, crystal planes, structures and orientation, and the mechanical characteristics of IN718. The 1 h of homogenization at 1080° C did not make any modification to the as-built grain texture and orientation. Uriati and Nicoletto111 examined the fatigue behavior of Inconel 718 with three L-PBF industrial systems through variations in layer thicknesses. Miniature specimens were for researching fatigue behavior. Surface roughness was measured using contact and optical profilometers.

The results of the tests defining fatigue scatter could be used for assisting designers in the creation of L-PBF Inconel 718 parts. Surface orientation had an effect on the fatigue behavior of IN718 on as-built surfaces. The directional fatigue strength ranged from 280 to 450 MPa after 2 million cycles. Variability in fatigue performance due to AM equipment and process parameters led to an optimization study for a reduction in postprocessing on surfaces. Yu et al.112 examined the fatigue life using an ultrasonic fatigue test for assessment of the impact of sandblasting and HIP of PBF-IN718. Kurtosis was used for evaluation of surface status due to its characterization of it defect morphology. Sandblasting and sandblasting with HIP have a significant impact on AM tensile characteristics. Very high cycle fatigue (VHCF) resistance was affected by the surface condition and microdefects. Kurtosis, rather than arithmetic mean height, better characterizes fault morphology.

Yan et al.113 fabricated the Inconel 625 specimens' samples with three distinct orientations (0°, 45°, and 90°). Columnar dendrites and equiaxed grains made a majority of the surface microstructure of the fabricated specimens. The SLM 45° specimen had the most significant value for surface roughness compared with other areas. According to the remelting phenomena, the SLM 0° specimens also had the smoothest surface. In contrast, the SLM 45° samples had the uneven surface due to the bead up and stair-stepping effects. According to Lesyk et al.,114 the turbine blade test specimens were made with IN-718 powder. Mechanical post-treatment methods such as Barrel Finishing (BF), Shot Peening (SP), Ultrasonic Shot Peening (USP), and Ultrasonic Impact Treatment (UIT) were used for enhancing SLM-built specimen near-surface region characteristics. After BF, USP, and UIT, surface roughness of 5.27 μm reduced by 20%, 6%, and 57.4%. After BF, USP, and UIT operations, near-surface layers are 80 to 180 μm thick and 140 to 180 μm thick after SP, UIT, and SP treatments.

A study by Wan et al.115 showed that after surface machining and polishing, which decreased the surface roughness Ra from 14 μm to 110 nm, the fatigue strength of Inconel 718 produced by SLM was increased by 50% at 650°C. Thinner, unmachined specimens show longer fatigue lifetimes than thicker ones, but machined specimens show the opposite trend. Substantial stress concentrations lead to a pronounced influence of defect shape on fatigue properties than the defect depth when the defect depth is smaller than 200 μm. Zhang and Fatemi116 examined SLM Inconel 718 sample post-treatment, such as various HTs and electrochemical polishing. Following HT1200 treatment, samples exhibited very low pitting corrosion resistance. The thick oxide coating produced on the surface during the electropolishing process provided a sizeable passive zone, which raised the critical pitting potential.

Majeed et al.117 investigated the surface quality SLM products through variations in the process parameters and postprocessing techniques. There was an increase in surface roughness of the specimen with an increase in the laser energy level. However, 0.32 kW laser power produced the most significant results. After being heated in solution at 540°C for 2 h, most samples (77%) had minor surface roughness on average. Artificial aging at 155°C for 12 h, primarily at 530°C, and optimum parameters for the highest surface quality in the as-built condition were 0.60 m/s scanning rate, overlapping percentage of 35%, and 88.7 mm of hatch spacing.

Titanium alloys

Ahmed et al.118 used the material Ti–5Al–5Mo–5V–3Cr (wt. %) for their work due to its remarkable properties in obtaining better surface quality processing parameters, scanning rate and laser energy are varied. The manufactured coupons had a surface roughness (Sa/Ra) of <20 μm. Semifused powder particles, open pores on the surface, microcracks, and cracks formed on the interlayer could all be perceived on the cross-sectional surface. Regardless of the laser power utilized in this study, specimens fabricated by the scanning rate of 1200 mm/s improved surface properties. Alejandro et al.119 fabricated additively manufactured millimeter sized component and analyzed using X-ray computed tomography (XCT) technique. Ti-6Al-4V struts were created using electron beam melting (EBM) at 45° and vertical inclinations. The volume and size of partially melted particles and the cross-sectional shape of the strut were measured in depth.

The increased roughness on the specimens' lateral surfaces was unusual. Roughness variations were minimal but apparent in vertically produced struts. Mondal et al,120 examined the bone tissue engineering and orthopedics use porous structures of titanium alloy. SLM created porous scaffolds with complex internal and exterior shapes, enabling SLM to be one of the most influential biomedical manufacturing methods. SLM scaffolds offered great pore precision and poor mechanical strength. Grid-type structures were seen having relatively low surface roughness and improved production capability, with fewer porosity defects. Kaierle et al.121 fabricated titanium alloy with PBF related to high as-built surface roughness and texture. Processing parameters were seen as affecting surface roughness and porosity. This study was related to the effect of residual oxygen on virgin and recycled powder porosity. Recycled powder was seen as rougher than virgin powder. The surface texture depends on scan direction and energy input.

Adherence of particles on the side caused increase in surface roughness. Recycling powder or residual oxygen did not have any effect on surface roughness. Pedro et al.122 investigated the VHCF regimen on the PBF of titanium alloy Ti6Al4V. While polished specimens featured subsurface cracks, as-built specimens showed cracks in the beginning of a surface. This study made an assessment of the effects of defect size, position, surface finish, and defects and roughness on the fatigue strength. Surface roughness, fatigue stress life, and fracture surface were examined between as-built and polished surfaces. Surface roughness as-built led to cracking. Ti6Al4V SLM samples were subjected to ultrasonic fatigue testing without any HT. The results of the fatigue fracture correspond to VHCF data that have already been published. Reduced fatigue strength was caused by variations in fracture surface shape and no interior crack initiation.

Dareh et al.123 designed a new model for facilitating the SLM production of straight undistorted horizontal pieces without postprocessing. Horizontally built titanium grade 5 specimens were compared with vertically built specimens in their as-print condition. Vertical samples fracture prematurely, but horizontal sections execute equally to post-treated samples. The fracture stress of the as-printed vertical sections is <38% of the ultimate tensile strength (UTS). Ti-6Al-4 V vertical samples break at 38% of their horizontal counterparts' nominal load. This problem is assumed to be related to vertical as-built surface inadequacies, which can be correlated to surface quality and RS. Sanaei and Fatemi124 investigated the impact of surface finish and surface roughness on the fatigue life of samples produced using PBF with titanium grade 5 powder. Internally flawed PBF specimens with martensitic and lamellar microstructures and HIPed specimens with much coarser microstructures and reduced interior defects were used for collection of data on fatigue.

The effect of surface roughness and internal flaws on fatigue performance of PBF Ti-6Al4Vs was examined. Even in the presence of relatively severe internal faults, the influence of surface roughness was negative and predominant in fatigue performance. The secondary effects of internal flaws and microstructure on the scatter of stress life data of machined surface specimens were also investigated. According to Li et al.125 SLM is a potential rapid implantation method for specialized dental implants using titanium alloy. High and uneven roughness on the surface of the implant created by SLM has a significant impact on osseointegration and early cell behaviors. In their study, samples were created using various inclination degrees. Difference in inclination angles impact surface roughness, owing to sthe taircase effect and the heat-affected zone. The implant produced with parameters showed a low and stable roughness compared with the implant manufactured with a single-parameter method.

Yánez et al.126 made a study of the impact of surface finish and surface roughness on the fatigue life of titanium grade 5 alloy structures made of gyroid cells. Stress peak sites were found on the stress concentrators, due to surface flaws. Micrographs taken using a scanning electron microscope revealed the surface where the crack began to form. The superficial roughness contributing to the notch effect was seen having a negative impact on the expected favorable fatigue behavior caused by the curvature in the strut joints. Günther et al.127 assessed the fatigue properties of samples having rough as-built internal axial channel surfaces due to limited accessibility. Variable-diameter and channel-count samples did not always show worse fatigue performance than solid samples. The S-N curve shows fatigue behavior and shows how surface roughness and porosity affect it. Internal roughness in SLM Ti-6Al-4V was tolerated for applications requiring 300 MPa fatigue strength.

Enhanced fatigue performance requires coupled outer/inner surface smoothing and HIP compaction. Khorasani et al.128 analyzed the LPBF-titanium alloy samples by varying the process parameters and postprocessing techniques. Enhanced heat transfer rate and melting pool dynamics were investigated with the relationship between measured parameters and related mechanisms. There was an increase in temperature and particle size and a reduction in hardness. SR enhanced the hardness of samples with a lower energy density due to reduced α′ martensite.

Lerebours et al.129 examined the influence of surface texture variety on osteoblastic linage (MC3T3) cell adhesion and morphology utilizing a multidimensional stem-like sample generated with the use of PBF technique of titanium grade 5 alloy. Microscale grooves improved cell adherence, but partially melted particles were the worst. Osteoblastic cells prefer skin surfaces with a slight slope, with less partially melted particles (entirely covered by particles). Ti6Al4V powder and as-built sample revealed the absence of subsidiary cytotoxicity.

Aluminum alloys

Fielden-Stewart et al.130 used the SLM technique for fabrication of aluminum alloy with different printing angles for analysis of the fracture toughness of hybrid joints. There was an increase in the roughness of the upper surface with an increase in the printing angle, whereas the bottom surface displayed the reverse tendency. Increase in the surface roughness of SLM caused an increase in polymer adhesive adhesion. Polishing and abrading SLM components after fabrication are counterproductive for bonded junctions. Geometry can be used for optimization of adhesion by adjusting the roughness of bonding surfaces. According to Plessis and Beretta,131 AM produces complicated components for aircraft applications. Surface roughness and finish, micrograph, RS, and porosity have effect on fatigue properties of the additively produced metal components. Surface “killer notches” are evaluated and contrasted to nearby roughness notches and pores.

A numerical study of the stress intensity factor and fatigue behavior data of identical samples validates these notches. Micro-CT data of as-built AlSi10Mg specimens were used for quantification of surface notches. The technique precisely forecasts seven failure positions through four failures at nonhighest stress intensity factor locations. Notches deeper than 50 μm can initiate cracks regardless of surface. Mohammadi and Asgari132 analyzed that the surface roughness of additively produced aluminum alloy AlSi10Mg 200C requires postprocessing such as bead blasting or machining. The surface of Sample 1 with greater skin energy density with a beam offset of 0.15 mm had better surface quality of 0.174% surface porosity level than a regular surface of Sample 2, with the same energy density but smaller beam offset of 0.1 mm which has produced the best direct metal laser sintering (DMLS)-AlSi10Mg 200C surface with 0.123% surface porosity level.

Maamoun133 analyzed the surface morphologies through varying the energy densities in AlSi10Mg samples. The variations are shown in Figure 10 through scanning electron microscope (SEM) and 3D surface morphology examination. Lower energy density (ED) shows the balling effect with higher pores, mid-range of ED depicts the pores through improper melting of metal powders, whereas higher ED reveals a significant enhancement in surface quality by mitigating the pores and balling effect.

FIG. 10.

FIG. 10.

Surface morphologies of AlSi10Mg samples at different energy densities. (a, d, g) 65 J/mm3, (b, e, i) 50 J/mm3, (c, f, j) 65 J/mm3, (h) 40.5 J/mm3. (a–c) SEM observation at 50 × Magnification, (d–f) SEM observation at 100 × magnification, (g–j) 3D surface texture.

Copper alloys

According to Seltzman and Wukitch,134 lower hybrid current drive (LHCD) radio frequency (RF) launchers can be additively manufactured using the SLM 3D printing technique using the novel material GRCop84 copper. Surface roughness causes conditioning hindrance to increase in RF losses due to its trapping gas and impurities that cause arcing by emerging at high power from the surface. The anisotropic nature of the etch rates in SLM produced GRCop-84, leading to the requirement of etch period keeping to a minimum to avoid pitting that corresponds to the laser hatch pattern. After 20 min of etching, most adhered particles on the as-printed side wall coupon are successfully eliminated. However, it takes 40 min of etching to completely remove all the remaining adhered particles, although noticeable surface pitting becomes apparent.

Favero et al.135 analyzed the new possibilities in heat transfer that have been opened up by metal AM. Surface roughness has influence on the performance of a device. Numerical models require calibration for successful design due to the effect of surface roughness on fluid flow. Straight channel forecasts can be produced accurately with a relative variation that is nonsignificant for Re >30,000 and more than acceptable at lower Reynolds numbers. Forecasts of channel fluid flow performance can be inaccurate, as this research demonstrates, when numerical tool calibration is not performed. According to Nicoletto et al.,136 miniature specimens with varying build direction orientations were used for the assessment of the fatigue behavior of heat-treated DMLS and EBM Ti6Al4V.

Review of results was based on as-built surface characterization and earlier investigations on the same material. DMLS Ti6Al4V was seen as a higher fatigue strength than EBM Ti6Al4V and DMLS Ti6Al4V a smoother surface than EBM. The directional fatigue results of both technologies were seen with difference, and surface roughness and morphology were different. Ramanathan et al.137 investigate IN-718 alloy with EBM and SLM. Aerospace and gas turbine sectors are interested in EBM and SLM for topology-optimized designs, lattice parts, and part consolidation. SLM material fatigue qualities approach wrought material, but EBM flaws affect fatigue life. EBM as-built surface roughness is three times SLM. Crack propagation looks more ductile for HT material versus HIP+HT.

A thorough examination of surface finish and roughness revealed the direct effect of the roughness parameter on fatigue behavior, where the roughness introduces the irregularities in the surface that act as stress concentrators, leading to the initiation and propagation of fatigue cracks. Compared with the laser parameters, the built parameters, scanning speed, vertical orientation, higher laser power, and scanning strategies impact the surface finish and roughness of the additively manufactured samples. Thermal postprocessing procedures do not have any influence on surface finish and roughness. The 45° and 60° orientations minimize roughness for flat specimens and other three-dimensional or complex models.

The recycled powder has a higher roughness than the virgin powder, but it does not result in a higher roughness during specimen fabrication. Sandblasting, electropolishing, barrel finishing, shot peening, ultrasonically assist shot peening, ultrasonic impact peening, surface remelting, and magnetic field-assisted polishing for a reduction in the surface roughness and improve the surface finish of additively fabricated specimens.

Recent Advancements in PBF

In recent years, there have been several advancements in PBF AM that have improved the technology and its capabilities. Here are a few examples:

  • Multilaser systems: Multilaser systems use multiple lasers to melt and fuse the metal powders, which can improve the speed and efficiency of the PBF AM build process.

  • In situ monitoring: In situ monitoring systems are used to monitor the PBF AM process in real time, which allows for improved process control and the ability to detect and correct any issues that may arise during the build process.

  • Automated postprocessing: Automated postprocessing systems are used to remove support structures, to enhance smooth surfaces, and to achieve the desired properties. This can save time and cost and improve the quality of the final product.

  • Hybrid manufacturing: Hybrid manufacturing combines traditional manufacturing techniques, such as milling and turning, with PBF AM to create complex geometries, internal structures, and smooth surface finish, which is not possible with PBF alone.

  • Materials development: The development of new alloys and metal powders suitable for PBF AM has been a major focus in recent years. This allows for the creation of parts with new properties and improved performance.

  • Quality control: The development of in-process quality control systems has been a significant advancement in PBF AM. This allows for the real-time monitoring of the process, the detection of defects, and the ability to correct it during the build process.

These advancements have led to improved efficiency, precision, and accuracy in PBF AM, and have opened up new possibilities for the use of this technology in various industries.

Defects in WAAM

WAAM is a technological advancement in metal AM, which also provides a faster production rate, and the solidification rate in WAAM is not necessarily faster compared with other metal AM processes. The solidification rate can vary depending on several factors such as the specific parameters used, the geometry of the part, and the material being used. However, the defects formed in WAAM due to a variety of factors, including incomplete fusion, improper process control, porosity, and contaminants. In this section, the defect formation mechanisms underlying each of these considerations are discussed in detail.

Akgun et al.138 analyzed the fracture surface in wire-arc additive manufactured Ti-6Al-4V with three induced pore types: embedded pore, surface pore, and cluster pore. Evaluation of the fatigue life and cracks was analyzed through three types of induced pores with the micron scale. The increase in the fracture rate and a decrease in fatigue life were observed, when the pore size was increased beyond 85 μm. Aldalur et al.139 compared and investigated the gas metal arc-based WAAM cold arc technique, pulsed AC mode, and pulsed gas metal arc welding (GMAW) AC mode with manufactured Al-Mg alloys. The absence of microstructural changes and a high penetration depth in all three modes were observed. A reduction in porosity in pulsed AC mode was observed, when compared with other modes due to variable polarity in the process.

Fu et al.140 utilized the hot WAAM technique for a reduction in two primary defects, namely, porosity and an increased deposition rate in aluminum alloy. Hot-WAAM was introduced for printing four samples with different parameters to overcome the issues. By increasing the hot-wire current, a substantial decrease in the total energy input per unit volume was observed, reducing it from 84.0 J/mm3 to 40.1 J/mm3. Concurrently, the deposition rate exhibited an exponential increase, soaring from 86 to 301 cm3/h. However, this escalated deposition rate resulted in a compromised macrostructure and surface quality, indicating a trade-off. Notably, the introduction of hot-wire assistance led to a significant reduction in porosity. The density reached an impressive 99.646% when the hot-wire current was set to 100 A. It was observed that the pores were primarily concentrated on the interlayer region, which coincided with the top of the melt pool.

Wang et al.141 observed that the porosity was increased by increasing the deposition rate due to incomplete fusion when they manufactured the mobile heat storage equipment using WAAM of Al alloy. Rajkumar et al.142 manufactured Incoloy 825 and determined that it had superior corrosion resistance ranging around 0.59 and 0.70 mpy with better microhardness. They utilized it in offshore applications. Whereas with a range of 0.18 and 0.21 mm/year, Vishnukumar et al.143 assessed the superior corrosion resistance of the aluminum structures for saline applications through WAAM. Also, super-duplex SS with a range of 1.54 to 1.61 mpy was developed for petrochemical and coastal applications and tested for its significant corrosion resistance.15

Recent advancements in WAAM

WAAM has seen several notable advances in recent years that have significantly improved the capabilities and versatility of the technology. Some of the most notable advancements include the following:

  • Multiaxis systems: Developing multiaxis systems that allow for more freedom in the movement of the filler wire, enabling the creation of more complex geometries and internal structures.

  • In situ sensing and control: Developing in situ sensing and control systems that provide real-time feedback on the process and allow for real-time adjustments to the process parameters, leading to improved precision and repeatability.

  • High-speed deposition: Developing high-speed deposition techniques that allow for faster build rates, enabling the creation of large-scale objects in a shorter amount of time.

  • Automated process control: Developing automated systems for controlling the filler wire and the position of the substrate, leading to improved precision and repeatability, as well as increased efficiency and automation of the process.

  • Multimaterials: Developing techniques for creating multimaterial objects by using multiple filler wires with different properties and compositions, such as combination of dissimilar materials, making the technology more versatile and suitable for different applications.

  • Hybrid systems: Combining WAAM with other AM methods, such as laser welding, to improve the quality of the final object and to overcome some of the limitations of the technology.

  • Postprocessing: Developing new techniques for postprocessing, such as polishing and HT, to improve the quality of the surface and mechanical characteristics of the final object.

  • Ultracold-WAAM (UC-WAAM): The study presents a new variant of WAAM called UC-WAAM. UC-WAAM uses an electric arc between the wire feedstock material and a nonconsumable tungsten electrode. The feasibility of UC-WAAM was investigated using high-strength low-alloy steel (HSLA) and compared with conventional GMAW-based WAAM. By eliminating the electric current through the substrate and adjusting the arc position, UC-WAAM achieves lower process temperatures and higher cooling rates without compromising part integrity or deposition rate. Mechanical testing demonstrated that UC-WAAM maintains the high mechanical strength and ductility of the HSLA steel parts. The study also highlights a unique feature of UC-WAAM, which involves using a nonconductive/nonmetallic block to create overhang structures, showcasing its potential for fabricating complex-shaped 3D structures without additional support.19

  • Shape memory alloys: The study explores the fabrication of NiTiTa shape memory alloys through WAAM for the first time. The feedstock materials consisted of commercially available NiTi wire and Ta foil. The incorporation of Ta had a notable impact on the phase transformation temperatures, resulting in a room-temperature microstructure that included B19’ martensite, B2 austenite. Furthermore, the WAAM fabricated NiTiTa material demonstrated stable super elastic behavior throughout ten loading–unloading cycles, signifying its potential suitability for biomedical applications. This study introduces an innovative method for additively manufacturing NiTi-based multicomponent shape memory alloys using WAAM.6

Overall, these remarkable advances in WAAM have significantly expanded the capabilities of the technology, making it more versatile and suitable for a wide range of applications, and have led to improved precision, repeatability, and quality of the final object.

Economic Implications of Defect Reduction in AM Products

Reducing defects in metal AM can have a significant impact on the economics of the manufacturing process.

  • First, the cost of materials can be reduced as less metal is wasted due to defects, which can be a significant cost savings for metal AM, as metal is typically more expensive than other materials.

  • Second, high productivity can be achieved, when the parts are produced in a shorter amount of time, thus reducing the labor costs.

  • Third, it can also increase the yield of the process, resulting in more salable parts and thus increasing the revenue.

  • Lastly, it can also decrease the amount of rework needed on parts, reducing the costs associated with postprocessing, inspection, and quality control.

In a study conducted by Kokare et al.,144 the economic and environmental aspects of WAAM, PBF, and CNC milling techniques were investigated and compared. It was found that the CNC milling demonstrated the best balance between cost-effectiveness and ecological impact, followed by WAAM and PBF. Overall, reducing defects in metal AM can lead to a number of economic benefits, including reduced costs, increased productivity, and revenue. However, the performance of each process depends on factors such as product complexity and material efficiency. This can make the manufacturing process more cost-effective, and thus more competitive in the market.

Challenges and Future Perspectives

Prospects for further and the most significant difficulties seen in the field of metal AM of various alloys are summarized:

  • Material properties: The biggest challenges in metal AM are ensuring that the properties of the final product match the properties of the metal powder or alloy used. Due to the nature of the AM process, the microstructure and properties of the final product can be different from those of conventionally manufactured parts. This can result in variations in strength, ductility, and toughness.

  • Material selection: Selecting the right alloy for a specific application can be challenging as different alloys have different properties and are suitable for different types of products and manufacturing processes. In addition, not all alloys are currently available in powder form for use in metal AM.

  • Powder production: Producing high-quality powders for metal AM is a complex process and can be challenging. Factors such as particle size, shape, and flowability can greatly impact the quality of the final product.

  • Surface quality: Another challenge in metal AM is achieving a smooth surface finish and minimal surface defects. The surface finish of the final product can be affected by factors such as the size and shape of the powder particles, flow rate, and the laser power. This can lead to surface roughness, porosity, and other defects. Deliberation on different materials and newly developed alloy materials on the surface and subsurface region is required for their fatigue behavior, surface roughness, and finish owing to flaws by the influence of the parametric method.

  • HT: Many metal alloys require HT for optimal properties and this process can be challenging with AM parts. The geometry and size of the parts can make it difficult to apply HT uniformly throughout the part. Also, the quantitative analysis of precipitates and the relationship between phase change and mechanical characterization on various materials is required.

  • Part size and complexity: Metal AM can be used to create parts with complex geometries, but the size of the parts is still limited. Some of the current AM machines have a maximum build volume that can be limiting to some applications.

  • Cost: Metal AM is still more expensive than traditional manufacturing methods, particularly for small-batch production. The cost of the raw materials, the machines, and the maintenance can be high.

  • Postprocessing: Metal AM parts often require postprocessing to remove support structures, smooth surfaces, and to achieve the desired properties. This can be time-consuming and costly.

  • Inspection and quality control: In-process inspection and quality control are challenges in metal AM. The process of AM does not allow for easy in-process inspection and it can be difficult to ensure that the final product meets the desired specifications.

  • Process control: Controlling the AM process can be difficult, as factors such as laser power, flow rate of the powder, and layer thickness can greatly impact the quality of the final product. Use of machine learning and artificial intelligence in built during an optimization-based method and model is required as per defect mitigation

  • Safety: Metal AM can pose safety risks, as the process involves the use of high-powered lasers and metal powders. Proper safety measures must be taken to minimize the risk of accidents and injuries.

  • Standards and regulations: The ASTM offers comprehensive standards covering various aspects of AM, including applications, design, materials and processes, terminologies, and test methods.145–151 For instance, ISO_ASTM52950-21 provides an overview of general principles and data processing in AM. ISO_ASTM52911-1-19 serves as a design guide specifically for laser-based PBF of metals. F3413-19e1 offers valuable insights as a design guide for AM using DED. Furthermore, F3184-16 specifies the standard requirements for AM of stainless-steel alloy (UNS S31603) using PBF. These are just a few examples of the wide range of ASTM standards that provide detailed guidance and specifications for different aspects of AM. However, there is a lack of standardization and regulations for metal AM, which can make it difficult for manufacturers to ensure that their products meet industry standards and requirements in the way of fabrication and testing.

  • Lack of skilled personnel: As metal AM is a relatively new technology, there is a shortage of skilled personnel who are able to operate and maintain the machines, as well as design and optimize parts for the process.

  • Examination of the mitigation of stress concentration and stiffness during prefabrication and postfabrication on irregular geometries, lattice structures, gradient lattice structures, unit cells, and metamodels with thin and curvilinear struts is required.

Whereas while metal AM has the potential to revolutionize the way metal parts are designed, manufactured, and used, there are still many challenges that must be overcome before it can be fully adopted and utilized in various industries. These challenges include material properties, surface quality, HT, part size and complexity, cost, postprocessing, inspection and quality control, material selection, powder production, process control, safety, standards and regulations, and lack of skilled personnel.

Summary

The in-depth study analyses of the primary contributing variables to the development of defects, and the control strategies, mechanisms, and analytical models for the formation of defects in components manufactured by the PBF process and other processes are summarized as follows:

  • (1)

    The most commonly used alloys are titanium, steel, Inconel, and aluminum due to their unique combination of strength and durability. In the area of mechanical characteristics, titanium alloys exhibit the best performance, while steel alloys have demonstrated for improved resistance to corrosion and strength. When it comes to common defects, alloys copper and tungsten have found to be prone to cracking due to high thermal conductivity, while the aluminum alloy has a higher tendency toward warping.

  • (2)

    High scanning rate, lower laser power, toolpath strategy, grain refinement, and laser scattering increase the porosity and degrading mechanical characteristics. Porosity is minimized through process parameter optimization and different postprocessing techniques.

  • (3)

    At higher and lower VED, uneven laser track, lower overlapping percentage, keyhole and LoF pores are generated. Optimization of the process parameters, the remelting of the layer, and subsequent grain refining by postprocessing processes helps to reduce the LoF porosity.

  • (4)

    Balling can be reduced through optimization of the process parameters and rescanning the built layer with a higher VED, overlapping laser tracks, and an overlay region.

  • (5)

    The SLM method produces higher RS than the DED process, which generates less RS. Compressive RS in the interface zone between the SLM and DED techniques is superior. It is possible to reduce RS using thermal postprocessing processes and DCT.

  • (6)

    The roughness parameter has direct impact on fatigue behavior following a thorough investigation of surface finish and roughness. Forty-five-degree and 60° orientations reduce roughness on flat specimens and other three-dimensional or complex models with surface post-treatment techniques such as peening and surface remelting.

During the PBF-based and other AM processes, the above-analyzed factors and postprocessing techniques are seen to prevent, reduce, and at least minimize the occurrence of defects in the final product's precision, irregularity, and finish to enhance the mechanical and material characteristics.

Data Availability

No data were used for the research described in the article.

Authors' Contributions

R.H.: writing—review and editing, writing—original draft, visualization, conceptualization, formal analysis, and data curation. T.S.K.: methodology, investigation, formal analysis, data curation, and supervision.

Author Disclosure Statement

The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this article.

Funding Information

No funding was received for this article.

References

  • 1. Zhai Y, Lados DA, Lagoy JL. Additive manufacturing: Making imagination the major limitation. JOM 2014;66(5):808–816; doi: 10.1007/S11837-014-0886-2/TABLES/2 [DOI] [Google Scholar]
  • 2. Vafadar A, Guzzomi F, Rassau A, et al. Advances in metal additive manufacturing: A review of common processes, industrial applications, and current challenges. Appl Sci 2021;11(3):1213. [Google Scholar]
  • 3. Revilla-León M, Meyer MJ, Özcan M. Metal additive manufacturing technologies: Literature review of current status and prosthodontic applications. Int J Comput Dent 2019;22(1):55–67. [PubMed] [Google Scholar]
  • 4. Trevisan F, Calignano F, Aversa A, et al. Additive manufacturing of titanium alloys in the biomedical field: Processes, properties and applications. J Appl Biomater Funct Mater 2018;16(2):57–67. [DOI] [PubMed] [Google Scholar]
  • 5. Li S, Li JY, Jiang ZW, et al. Controlling the columnar-to-equiaxed transition during Directed Energy Deposition of Inconel 625. Addit Manuf 2022;57:102958; doi: 10.1016/j.addma.2022.102958 [DOI] [Google Scholar]
  • 6. Zuo X, Zhang W, Chen Y, et al. Wire-based directed energy deposition of NiTiTa shape memory alloys: Microstructure, phase transformation, electrochemistry, X-ray visibility and mechanical properties. Addit Manuf 2022;59(PB):103115; doi: 10.1016/j.addma.2022.103115 [DOI] [Google Scholar]
  • 7. Li B, Wang L, Wang B, et al. Electron beam freeform fabrication of NiTi shape memory alloys: Crystallography, martensitic transformation, and functional response. Mater Sci Eng A 2022;843:143135; doi: 10.1016/j.msea.2022.143135 [DOI] [Google Scholar]
  • 8. Ligon SC, Liska R, Stampfl J, et al. Polymers for 3D printing and customized additive manufacturing. Chem Rev 2017;117(15):10212–10290. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 9. Saleh Alghamdi S, John S, Roy Choudhury N, et al. Additive manufacturing of polymer materials: Progress, promise and challenges. Polymers (Basel) 2021;13(5):753. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 10. Gorsse S, Hutchinson C, Gouné M, et al. Additive manufacturing of metals: A brief review of the characteristic microstructures and properties of steels, Ti-6Al-4V and high-entropy alloys. Sci Technol Adv Mater 2017;18(1):584–610. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 11. ISO/ASTM International. Additive manufacturing—General principles terminology (ASTM52900). Rapid Manuf Assoc 2013;2021:10–12. [Google Scholar]
  • 12. Angrish A. A Critical Analysis of Additive Manufacturing Technologies for Aerospace Applications. In: 2014. IEEE Aerospace Conference, 01–08 March 2014. Big Sky, MT, USA, 2014; pp. 1–6. [Google Scholar]
  • 13. Körner C. Additive manufacturing of metallic components by selective electron beam melting—A review. Int Mater Rev 2016;61(5):361–377. [Google Scholar]
  • 14. Singh DD, Mahender T, Reddy AR. Powder bed fusion process: A brief review. Mater Today Proc 2021;46:350–355. [Google Scholar]
  • 15. Rajesh Kannan A, Siva Shanmugam N, Rajkumar V, et al. Insight into the microstructural features and corrosion properties of wire arc additive manufactured super duplex stainless steel (ER2594). Mater Lett 2020;270:127680; doi: 10.1016/j.matlet.2020.127680 [DOI] [Google Scholar]
  • 16. Prakash KS, Kannan AR, Pramod R, et al. Microstructure, mechanical properties and fracture toughness of SS 321 stainless steel manufactured using wire arc additive manufacturing. Trans Indian Inst Met 2023;76:537–544; doi: 10.1007/s12666-022-02713-3 [DOI] [Google Scholar]
  • 17. Sasikumar R, Kannan AR, Kumar SM, et al. Wire arc additive manufacturing of functionally graded material with SS 316L and IN625: Microstructural and mechanical perspectives. CIRP J Manuf Sci Technol 2022;38:230–242; doi: 10.1016/j.cirpj.2022.05.005 [DOI] [Google Scholar]
  • 18. Rajesh Kannan A, Mohan Kumar S, Pravin Kumar N, et al. Process-microstructural features for tailoring fatigue strength of wire arc additive manufactured functionally graded material of SS904L and Hastelloy C-276. Mater Lett 2020;274:127968; doi: 10.1016/j.matlet.2020.127968 [DOI] [Google Scholar]
  • 19. Rodrigues TA, Duarte VR, Miranda RM, et al. Ultracold-wire and arc additive manufacturing (UC-WAAM). J Mater Process Technol 2021;296:117196; doi: 10.1016/j.jmatprotec.2021.117196 [DOI] [Google Scholar]
  • 20. Rodrigues TA, Cipriano Farias FW, Zhang K, et al. Wire and arc additive manufacturing of 316L stainless steel/Inconel 625 functionally graded material: Development and characterization. J Mater Res Technol 2022;21:237–251; doi: 10.1016/j.jmrt.2022.08.169 [DOI] [Google Scholar]
  • 21. Bevans B, Ramalho A, Smoqi Z, et al. Monitoring and flaw detection during wire-based directed energy deposition using in-situ acoustic sensing and wavelet graph signal analysis. Mater Des 2023;225:111480; doi: 10.1016/j.matdes.2022.111480 [DOI] [Google Scholar]
  • 22. Kannan AR, Kumar SM, Pramod R, et al. Microstructure and corrosion resistance of Ni-Cu alloy fabricated through wire arc additive manufacturing. Mater Lett 2022;308(PB):131262; doi: 10.1016/j.matlet.2021.131262 [DOI] [Google Scholar]
  • 23. Pramod R, Mohan Kumar S, Girinath B, et al. Fabrication, characterisation, and finite element analysis of cold metal transfer-based wire and arc additive-manufactured aluminium alloy. Riv Ital della Saldatura 2021;73(3):331–350. [Google Scholar]
  • 24. Chahal V, Taylor RM. A review of geometric sensitivities in laser metal 3D printing. Virtual Phys Prototyp 2020;15(2):227–241. [Google Scholar]
  • 25. Snow Z, Nassar AR, Reutzel EW. Invited review article: Review of the formation and impact of flaws in powder bed fusion additive manufacturing. Addit Manuf 2020;36:101457. [Google Scholar]
  • 26. Echeta I, Feng X, Dutton B, et al. Review of defects in lattice structures manufactured by powder bed fusion. Int J Adv Manuf Technol 2020;106(5):2649–2668. [Google Scholar]
  • 27. Carlton HD, Haboub A, Gallegos GF, et al. Damage evolution and failure mechanisms in additively manufactured stainless steel. Mater Sci Eng A 2016;651:406–414. [Google Scholar]
  • 28. Courtois M, Carin M, Le Masson P, et al. A two-dimensional axially-symmetric model of keyhole and melt pool dynamics during spot laser welding. Metall Res Technol 2013;110(2):165–173. [Google Scholar]
  • 29. Haribaskar R, Kumar TS, Tamiloli N. Surface integrity of additively manufactured Inconel-718 by peening approaches. Mater Manuf Process 2023;38:1009–1019; doi: 10.1080/10426914.2022.2146716. [DOI] [Google Scholar]
  • 30. Barath Kumar MD, Aravindan KM, Vinoth Jebaraj A, et al. Effect of post-fabrication treatments on surface residual stresses of additive manufactured stainless steel 316L. FME Trans 2020;49(1):87–94; doi: 10.5937/FME2101087B [DOI] [Google Scholar]
  • 31. Jebaraj AV, Kumar TS, Kumar LA, et al. Influence of shot peening on surface quality of austenitic and duplex stainless steel. IOP Conf Ser Mater Sci Eng 2017;263(6):062057; doi: 10.1088/1757-899X/263/6/062057 [DOI] [Google Scholar]
  • 32. Kruth J-P, Froyen L, Van Vaerenbergh J, et al. Selective laser melting of iron-based powder. J Mater Process Technol 2004;149(1–3):616–622; doi: 10.1016/j.jmatprotec.2003.11.051 [DOI] [Google Scholar]
  • 33. Casavola C, Campanelli SL, Pappalettere C.. Experimental Analysis of Residual Stresses in the Selective Laser Melting Process. In: Proccedings of the XIth International Congress and Exposition, Orlando, FL, 2008. [Google Scholar]
  • 34. Mercelis P, Kruth J-P. Residual stresses in selective laser sintering and selective laser melting. Rapid Prototyp J 2006;12(5):254–265. [Google Scholar]
  • 35. Watkins T, Bilheux H, An K, et al. Neutron characterization for additive manufacturing. Adv Mater 2013;171(3):23. [Google Scholar]
  • 36. Pegues JW, Shao S, Shamsaei N, et al. Fatigue of additive manufactured Ti-6Al-4V, Part I: The effects of powder feedstock, manufacturing, and post-process conditions on the resulting microstructure and defects. Int J Fatigue 2020;132:105358. [Google Scholar]
  • 37. Calignano F, Manfredi D, Ambrosio EP, et al. Influence of process parameters on surface roughness of aluminum parts produced by DMLS. Int J Adv Manuf Technol 2013;67(9):2743–2751. [Google Scholar]
  • 38. Gharbi M, Peyre P, Gorny C, et al. Influence of a pulsed laser regime on surface finish induced by the direct metal deposition process on a Ti64 alloy. J Mater Process Technol 2014;214(2):485–495. [Google Scholar]
  • 39. Linins O, Krizbergs J, Boiko I. Surface texture metrology gives a better understanding of the surface in its functional state. Key Eng Mater 2013;527:167–172. [Google Scholar]
  • 40. Rao GA, Prasad KS, Kumar M, et al. Characterisation of hot isostatically pressed nickel base superalloy Inconel* 718. Mater Sci Technol 2003;19(3):313–321. [Google Scholar]
  • 41. Ahmed Obeidi M, Uí Mhurchadha SM, Raghavendra R, et al. Comparison of the porosity and mechanical performance of 316L stainless steel manufactured on different laser powder bed fusion metal additive manufacturing machines. J Mater Res Technol 2021;13:2361–2374; doi: 10.1016/j.jmrt.2021.06.027 [DOI] [Google Scholar]
  • 42. Murphy-Leonard AD, Pagan DC, Callahan PG, et al. Investigation of porosity, texture, and deformation behavior using high energy X-rays during in-situ tensile loading in additively manufactured 316L stainless steel. Mater Sci Eng A 2021;810:141034; doi: 10.1016/j.msea.2021.141034 [DOI] [Google Scholar]
  • 43. Ball S, Ghayoor M, Pasebani S, et al. Statistical analysis of porosity and process parameter relationships in metal additive manufacturing. Proc Manuf 2021;53:343–347; doi: 10.1016/j.promfg.2021.06.037 [DOI] [Google Scholar]
  • 44. Tapia G, Elwany AH, Sang H. Prediction of porosity in metal-based additive manufacturing using spatial Gaussian process models. Addit Manuf 2016;12:282–290; doi: 10.1016/j.addma.2016.05.009 [DOI] [Google Scholar]
  • 45. Panwisawas C, Gong Y, Tang YT, et al. Additive manufacturability of superalloys: Process-induced porosity, cooling rate and metal vapour. Addit Manuf 2021;47:102339; doi: 10.1016/j.addma.2021.102339 [DOI] [Google Scholar]
  • 46. Babamiri BB, Indeck J, Demeneghi G, et al. Quantification of porosity and microstructure and their effect on quasi-static and dynamic behavior of additively manufactured Inconel 718. Addit Manuf 2020;34:101380; doi: 10.1016/j.addma.2020.101380 [DOI] [Google Scholar]
  • 47. Xiong Y, Han Z, Qin J, et al. Effects of porosity gradient pattern on mechanical performance of additive manufactured Ti-6Al-4V functionally graded porous structure. Mater Des 2021;208:109911; doi: 10.1016/j.matdes.2021.109911 [DOI] [Google Scholar]
  • 48. Muro-Barrios R, Cui Y, Lambros J, et al. Dual-scale porosity effects on crack growth in additively manufactured metals: 3D ductile fracture models. J Mech Phys Solids 2022;159:104727; doi: 10.1016/j.jmps.2021.104727 [DOI] [Google Scholar]
  • 49. Liu P, Yi K, Jeon I, et al. Porosity inspection in directed energy deposition additive manufacturing based on transient thermoreflectance measurement. NDT E Int 2021;122:102491; doi: 10.1016/j.ndteint.2021.102491 [DOI] [Google Scholar]
  • 50. Pappas JM, Dong X. Porosity characterization of additively manufactured transparent MgAl2O4 spinel by laser direct deposition. Ceram Int 2020;46(5):6745–6755; doi: 10.1016/j.ceramint.2019.11.164 [DOI] [Google Scholar]
  • 51. Lifton J, Liu T. An adaptive thresholding algorithm for porosity measurement of additively manufactured metal test samples via X-ray computed tomography. Addit Manuf 2021;39:101899; doi: 10.1016/j.addma.2021.101899 [DOI] [Google Scholar]
  • 52. Vargas-Uscategui A, King PC, Yang S, et al. Toolpath planning for cold spray additively manufactured titanium walls and corners: Effect on geometry and porosity. J Mater Process Technol 2021;298:117272; doi: 10.1016/j.jmatprotec.2021.117272 [DOI] [Google Scholar]
  • 53. Hamid M, Saleh MS, Afrouzian A, et al. Modeling of porosity and grain size effects on mechanical behavior of additively manufactured structures. Addit Manuf 2021;38:101833; doi: 10.1016/j.addma.2020.101833 [DOI] [Google Scholar]
  • 54. Khalil M, Teichert GH, Alleman C, et al. Modeling strength and failure variability due to porosity in additively manufactured metals. Comput Methods Appl Mech Eng 2021;373:113471; doi: 10.1016/j.cma.2020.113471 [DOI] [Google Scholar]
  • 55. Ning J, Sievers DE, Garmestani H, et al. Analytical modeling of part porosity in metal additive manufacturing. Int J Mech Sci 2020;172:105428; doi: 10.1016/j.ijmecsci.2020.105428 [DOI] [Google Scholar]
  • 56. Laleh M, Hughes AE, Yang S, et al. A critical insight into lack-of-fusion pore structures in additively manufactured stainless steel. Addit Manuf 2021;38:101762; doi: 10.1016/j.addma.2020.101762 [DOI] [Google Scholar]
  • 57. Ronneberg T, Davies CM, Hooper PA. Revealing relationships between porosity, microstructure and mechanical properties of laser powder bed fusion 316L stainless steel through heat treatment. Mater Des 2020;189:108481; doi: 10.1016/j.matdes.2020.108481 [DOI] [Google Scholar]
  • 58. Bruna-Rosso C, Demir AG, Previtali B. Selective laser melting finite element modeling: Validation with high-speed imaging and lack of fusion defects prediction. Mater Des 2018;156:143–153; doi: 10.1016/j.matdes.2018.06.037 [DOI] [Google Scholar]
  • 59. Shrestha S, Chou K. Formation of keyhole and lack of fusion pores during the laser powder bed fusion process. Manuf Lett 2022;32:19–23; doi: 10.1016/j.mfglet.2022.01.005 [DOI] [Google Scholar]
  • 60. dos Santos Paes LE, Pereira M, Xavier FA, et al. Lack of fusion mitigation in directed energy deposition with laser (DED-L) additive manufacturing through laser remelting. J Manuf Process 2022;73:67–77; doi: 10.1016/j.jmapro.2021.10.052 [DOI] [Google Scholar]
  • 61. Promoppatum P, Srinivasan R, Quek SS, et al. Quantification and prediction of lack-of-fusion porosity in the high porosity regime during laser powder bed fusion of Ti-6Al-4V. J Mater Process Technol 2022;300:117426; doi: 10.1016/j.jmatprotec.2021.117426 [DOI] [Google Scholar]
  • 62. Bustillos J, Kim J, Moridi A. Exploiting lack of fusion defects for microstructural engineering in additive manufacturing. Addit Manuf 2021;48(PA):102399; doi: 10.1016/j.addma.2021.102399 [DOI] [Google Scholar]
  • 63. Coeck S, Bisht M, Plas J, et al. Prediction of lack of fusion porosity in selective laser melting based on melt pool monitoring data. Addit Manuf 2019;25:347–356; doi: 10.1016/j.addma.2018.11.015 [DOI] [Google Scholar]
  • 64. Darvish K, Chen ZW, Pasang T. Reducing lack of fusion during selective laser melting of CoCrMo alloy: Effect of laser power on geometrical features of tracks. Mater Des 2016;112:357–366; doi: 10.1016/j.matdes.2016.09.086 [DOI] [Google Scholar]
  • 65. Mukherjee T, DebRoy T. Mitigation of lack of fusion defects in powder bed fusion additive manufacturing. J Manuf Process 2018;36:442–449; doi: 10.1016/j.jmapro.2018.10.028 [DOI] [Google Scholar]
  • 66. Tang M, Pistorius PC, Beuth JL. Prediction of lack-of-fusion porosity for powder bed fusion. Addit Manuf 2017;14:39–48; doi: 10.1016/j.addma.2016.12.001 [DOI] [Google Scholar]
  • 67. Liu Y, Tang M, Hu Q, et al. Densification behavior, microstructural evolution, and mechanical properties of TiC/AISI420 stainless steel composites fabricated by selective laser melting. Mater Des 2020;187:1–13; doi: 10.1016/j.matdes.2019.108381 [DOI] [Google Scholar]
  • 68. Gusarov AV, Yadroitsev I, Bertrand P, et al. Heat transfer modelling and stability analysis of selective laser melting. Appl Surf Sci 2007;254(4):975–979; doi: 10.1016/j.apsusc.2007.08.074 [DOI] [Google Scholar]
  • 69. Pal S, Lojen G, Hudak R, et al. As-fabricated surface morphologies of Ti-6Al-4V samples fabricated by different laser processing parameters in selective laser melting. Addit Manuf 2020;33:101147; doi: 10.1016/j.addma.2020.101147 [DOI] [Google Scholar]
  • 70. Gao P, Wang Z, Zeng X. Effect of process parameters on morphology, sectional characteristics and crack sensitivity of Ti-40Al-9V-0.5Y alloy single tracks produced by selective laser melting. Int J Light Mater Manuf 2019;2(4):355–361; doi: 10.1016/j.ijlmm.2019.04.001. [DOI] [Google Scholar]
  • 71. Liu S, Guo H. Balling behavior of selective laser melting (SLM) magnesium alloy. Materials (Basel) 2020;13(16):3632; doi: 10.3390/MA13163632 [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 72. Zhou X, Liu X, Zhang D, et al. Balling phenomena in selective laser melted tungsten. J Mater Process Technol 2015;222:33–42; doi: 10.1016/j.jmatprotec.2015.02.032 [DOI] [Google Scholar]
  • 73. Li R, Liu J, Shi Y, et al. Balling behavior of stainless steel and nickel powder during selective laser melting process. Int J Adv Manuf Technol 2012;59(9–12):1025–1035; doi: 10.1007/s00170-011-3566-1 [DOI] [Google Scholar]
  • 74. Yadroitsev I, Gusarov A, Yadroitsava I, et al. Single track formation in selective laser melting of metal powders. J Mater Process Technol 2010;210(12):1624–1631; doi: 10.1016/j.jmatprotec.2010.05.010 [DOI] [Google Scholar]
  • 75. Ladewig A, Schlick G, Fisser M, et al. Influence of the shielding gas flow on the removal of process by-products in the selective laser melting process. Addit Manuf 2016;10:1–9; doi: 10.1016/j.addma.2016.01.004 [DOI] [Google Scholar]
  • 76. Kumaran M, Senthilkumar V, Justus Panicker CT, et al. Investigating the residual stress in additive manufacturing of combined process in powder bed fusion and directed energy deposition. Mater Today Proc 2021;47:4387–4390; doi: 10.1016/j.matpr.2021.05.200 [DOI] [Google Scholar]
  • 77. Wu H, He D, Guo X, et al. A segmented heat source for efficiently calculating the residual stresses in laser powder bed fusion process. J Manuf Process 2022;79:206–218; doi: 10.1016/j.jmapro.2022.04.051 [DOI] [Google Scholar]
  • 78. Narvan M, Ghasemi A, Fereiduni E, et al. Part deflection and residual stresses in laser powder bed fusion of H13 tool steel. Mater Des 2021;204:109659; doi: 10.1016/j.matdes.2021.109659 [DOI] [Google Scholar]
  • 79. Williams RJ, Vecchiato F, Kelleher J, et al. Effects of heat treatment on residual stresses in the laser powder bed fusion of 316L stainless steel: Finite element predictions and neutron diffraction measurements. J Manuf Process 2020;57:641–653; doi: 10.1016/j.jmapro.2020.07.023 [DOI] [Google Scholar]
  • 80. Pant P, Salvemini F, Proper S, et al. A study of the influence of novel scan strategies on residual stress and microstructure of L-shaped LPBF IN718 samples. Mater Des 2022;214:110386; doi: 10.1016/j.matdes.2022.110386 [DOI] [Google Scholar]
  • 81. Watkins TR, Unocic KA, Peralta A, et al. Residual stresses and microstructure within Allvac 718Plus laser powder bed fusion bars. Addit Manuf 2021;47:102334; doi: 10.1016/j.addma.2021.102334 [DOI] [Google Scholar]
  • 82. Goel S, Neikter M, Capek J, et al. Residual stress determination by neutron diffraction in powder bed fusion-built Alloy 718: Influence of process parameters and post-treatment. Mater Des 2020;195:109045; doi: 10.1016/j.matdes.2020.109045 [DOI] [Google Scholar]
  • 83. Nadammal N, Mishurova T, Fritsch T, et al. Critical role of scan strategies on the development of microstructure, texture, and residual stresses during laser powder bed fusion additive manufacturing. Addit Manuf 2021;38:101792; doi: 10.1016/j.addma.2020.101792 [DOI] [Google Scholar]
  • 84. Sirin TB, Kaynak Y. Prediction of residual stress and distortion in laser powder bed fusion additive manufacturing process of Inconel 718 alloy. Proc CIRP 2021;99:330–335; doi: 10.1016/j.procir.2021.03.102 [DOI] [Google Scholar]
  • 85. Wang X, Chou K. The effects of stress relieving heat treatment on the microstructure and residual stress of Inconel 718 fabricated by laser metal powder bed fusion additive manufacturing process. J Manuf Process 2019;48:154–163; doi: 10.1016/j.jmapro.2019.10.027 [DOI] [Google Scholar]
  • 86. Emanuelli L, Molinari A, Facchini L, et al. Effect of heat treatment temperature and turning residual stresses on the plain and notch fatigue strength of Ti-6Al-4V additively manufactured via laser powder bed fusion. Int J Fatigue 2022;162:107009; doi: 10.1016/j.ijfatigue.2022.107009 [DOI] [Google Scholar]
  • 87. Zhang CC, Wei HL, Liu TT, et al. Influences of residual stress and micro-deformation on microstructures and mechanical properties for Ti-6.5Al-3.5Mo-1.5Zr-0.3Si alloy produced by laser powder bed fusion. J Mater Sci Technol 2021;75:174–183; doi: 10.1016/j.jmst.2020.08.061 [DOI] [Google Scholar]
  • 88. Liu YG, Li MQ. Deformation mechanisms of nanocrystalline alpha titanium in Ti-6Al-4V. Mater Lett 2016;185:488–490; doi: 10.1016/j.matlet.2016.09.077 [DOI] [Google Scholar]
  • 89. Lan C, Wu Y, Guo L, et al. Microstructure, texture evolution and mechanical properties of cold rolled Ti-32.5Nb-6.8Zr-2.7Sn biomedical beta titanium alloy. J Mater Sci Technol 2018;34(5):788–792; doi: 10.1016/j.jmst.2017.04.017 [DOI] [Google Scholar]
  • 90. Cao S, Chu R, Zhou X, et al. Role of martensite decomposition in tensile properties of selective laser melted Ti-6Al-4V. J Alloys Compd 2018;744:357–363; doi: 10.1016/j.jallcom.2018.02.111 [DOI] [Google Scholar]
  • 91. Zhong HZ, Zhang XY, Wang SX, et al. Examination of the twinning activity in additively manufactured Ti-6Al-4V. Mater Des 2018;144:14–24; doi: 10.1016/j.matdes.2018.02.015 [DOI] [Google Scholar]
  • 92. Kumar VP, Jebaraj AV. Attainment of favorable microstructure for residual stress reduction through high-temperature heat treatment on additive manufactured inconel 718 alloy. Int J Adv Manuf Technol 2022;121(7–8):4455–4472; doi: 10.1007/s00170-022-09640-z [DOI] [Google Scholar]
  • 93. Levkulich NC, Semiatin SL, Gockel JE, et al. The effect of process parameters on residual stress evolution and distortion in the laser powder bed fusion of Ti-6Al-4V. Addit Manuf 2019;28:475–484; doi: 10.1016/j.addma.2019.05.015 [DOI] [Google Scholar]
  • 94. Pauzon C, Mishurova T, Evsevleev S, et al. Residual stresses and porosity in Ti-6Al-4V produced by laser powder bed fusion as a function of process atmosphere and component design. Addit Manuf 2021;47:102340; doi: 10.1016/j.addma.2021.102340 [DOI] [Google Scholar]
  • 95. Robinson J, Ashton I, Fox P, et al. Determination of the effect of scan strategy on residual stress in laser powder bed fusion additive manufacturing. Addit Manuf 2018;23:13–24; doi: 10.1016/j.addma.2018.07.001 [DOI] [Google Scholar]
  • 96. Zhou C, Sun Q, Qian D, et al. Effect of deep cryogenic treatment on mechanical properties and residual stress of AlSi10Mg alloy fabricated by laser powder bed fusion. J Mater Process Technol 2022;303:117543; doi: 10.1016/j.jmatprotec.2022.117543 [DOI] [Google Scholar]
  • 97. Sunny S, Mathews R, Yu H, et al. Effects of microstructure and inherent stress on residual stress induced during powder bed fusion with roller burnishing. Int J Mech Sci 2022;219:107092; doi: 10.1016/j.ijmecsci.2022.107092 [DOI] [Google Scholar]
  • 98. Marques DA, Oliveira JP, Baptista AC. A short review on the corrosion behaviour of wire and arc additive manufactured materials. Metals (Basel) 2023;13(4):641; doi: 10.3390/met13040641 [DOI] [Google Scholar]
  • 99. Mu J, Sun T, Leung CLA, et al. Application of electrochemical polishing in surface treatment of additively manufactured structures: A review. Prog Mater Sci 2023;136:101109; doi: 10.1016/j.pmatsci.2023.101109 [DOI] [Google Scholar]
  • 100. Liu Y, Wang X, Oliveira JP, et al. Spatial and directional characterization of wire and arc additive manufactured aluminum alloy using phased array ultrasonic backscattering method. Ultrasonics 2023;132:107024; doi: 10.1016/j.ultras.2023.107024 [DOI] [PubMed] [Google Scholar]
  • 101. Shen M, Kang C, Fang F. Material removal characteristics of various surface features on selective laser melted 316L stainless steel during electropolishing. J Manuf Process 2022;79:639–653; doi: 10.1016/j.jmapro.2022.04.072 [DOI] [Google Scholar]
  • 102. Yang K, Kim M, Kim D, et al. Investigation of laser powder bed fusion manufacturing and post-processing for surface quality of as-built 17-4PH stainless steel. Surf Coat Technol 2021;422:127492; doi: 10.1016/j.surfcoat.2021.127492 [DOI] [Google Scholar]
  • 103. Liang X, Dong W, Chen Q, et al. On incorporating scanning strategy effects into the modified inherent strain modeling framework for laser powder bed fusion. Addit Manuf 2021;37:101648; doi: 10.1016/j.addma.2020.101648 [DOI] [Google Scholar]
  • 104. Blinn B, Krebs F, Ley M, et al. Determination of the influence of a stress-relief heat treatment and additively manufactured surface on the fatigue behavior of selectively laser melted AISI 316L by using efficient short-time procedures. Int J Fatigue 2020;131:105301; doi: 10.1016/j.ijfatigue.2019.105301 [DOI] [Google Scholar]
  • 105. Wu P, Hirtler M, Bambach M, et al. Effects of build- and scan-directions on magnetic field-assisted finishing of 316L stainless steel disks produced with selective laser melting. CIRP J Manuf Sci Technol 2020;31:583–594; doi: 10.1016/j.cirpj.2020.08.010 [DOI] [Google Scholar]
  • 106. Sarkar S, Kumar CS, Nath AK. Effects of different surface modifications on the fatigue life of selective laser melted 155 PH stainless steel. Mater Sci Eng A 2019;762:138109; doi: 10.1016/j.msea.2019.138109 [DOI] [Google Scholar]
  • 107. Yamaguchi H, Fergani O, Wu P. Modification using magnetic field-assisted finishing of the surface roughness and residual stress of additively manufactured components. CIRP Ann 2017;66:305–308; doi: 10.1016/j.cirp.2017.04.084 [DOI] [Google Scholar]
  • 108. Portella Q, Chemkhi M, Retraint D. Influence of Surface Mechanical Attrition Treatment (SMAT) post-treatment on microstructural, mechanical and tensile behaviour of additive manufactured AISI 316L. Mater Charact 2020;167:110463; doi: 10.1016/j.matchar.2020.110463 [DOI] [Google Scholar]
  • 109. Detwiler S, Watring D, Spear A, et al. Relating the surface topography of as-built Inconel 718 surfaces to laser powder bed fusion process parameters using multivariate regression analysis. Precis Eng 2022;74:303–315; doi: 10.1016/j.precisioneng.2021.12.003 [DOI] [Google Scholar]
  • 110. Kumar Maurya A, Kumar A. Effect of building orientation & heat-treatment on microhardness & surface roughness of additive manufactured IN718 alloy. Mater Today Proc 2022;59:628–635; doi: 10.1016/j.matpr.2021.12.180 [DOI] [Google Scholar]
  • 111. Uriati F, Nicoletto G. A comparison of Inconel 718 obtained with three L-PBF production systems in terms of process parameters, as-built surface quality, and fatigue performance. Int J Fatigue 2022;162:107004; doi: 10.1016/j.ijfatigue.2022.107004 [DOI] [Google Scholar]
  • 112. Yu C, Huang Z, Zhang Z, et al. Effects of sandblasting and HIP on very high cycle fatigue performance of SLM-fabricated IN718 superalloy. J Mater Res Technol 2022;18:29–43; doi: 10.1016/j.jmrt.2022.02.077 [DOI] [Google Scholar]
  • 113. Yan X, Gao S, Chang C, et al. Effect of building directions on the surface roughness, microstructure, and tribological properties of selective laser melted Inconel 625. J Mater Process Tech 2021;288:116878; doi: 10.1016/j.jmatprotec.2020.116878 [DOI] [Google Scholar]
  • 114. Lesyk DA, Martinez S, Mordyuk BN, et al. Post-processing of the Inconel 718 alloy parts fabricated by selective laser melting: Effects of mechanical surface treatments on surface topography, porosity, hardness and residual stress. Surf Coatings Technol 2020;381:125136; doi: 10.1016/j.surfcoat.2019.125136 [DOI] [Google Scholar]
  • 115. Wan HY, Luo YW, Zhang B, et al. Effects of surface roughness and build thickness on fatigue properties of selective laser melted Inconel 718 at 650°C. Int J Fatigue 2020;137:105654; doi: 10.1016/j.ijfatigue.2020.105654 [DOI] [Google Scholar]
  • 116. Zhang J, Fatemi A. Surface roughness effect on multiaxial fatigue behavior of additive manufactured metals and its modeling. Theor Appl Fract Mech 2019;103:102260; doi: 10.1016/j.tafmec.2019.102260 [DOI] [Google Scholar]
  • 117. Majeed A, Ahmed A, Salam A, et al. Surface quality improvement by parameters analysis, optimization and heat treatment of AlSi10Mg parts manufactured by SLM additive manufacturing. Int J Light Mater Manuf 2019;2(4):288–295; doi: 10.1016/j.ijlmm.2019.08.001 [DOI] [Google Scholar]
  • 118. Ahmed M, Obeidi MA, Yin S, et al. Influence of processing parameters on density, surface morphologies and hardness of as-built Ti-5Al-5Mo-5V-3Cr alloy manufactured by selective laser melting. J Alloys Compd 2022;910:164760; doi: 10.1016/j.jallcom.2022.164760 [DOI] [Google Scholar]
  • 119. Alejandro Y, Hof LA, Vanderesse N, et al. On the characterization of roughness and geometrical irregularities of additively manufactured single titanium-alloy struts. 2022;54:102731; doi: 10.1016/j.addma.2022.102731 [DOI] [Google Scholar]
  • 120. Mondal P, Das A, Wazeer A, et al. Biomedical porous scaffold fabrication using additive manufacturing technique: Porosity, surface roughness and process parameters optimization. Int J Light Mater Manuf 2022;5(3):384–396; doi: 10.1016/j.ijlmm.2022.04.005 [DOI] [Google Scholar]
  • 121. Kaierle S, Emminghaus N, Hoff C. Residual oxygen content and powder recycling: Effects on surface roughness and porosity of additively manufactured Ti-6Al-4V. Addit Manuf 2021;46:102093; doi: 10.1016/j.addma.2021.102093 [DOI] [Google Scholar]
  • 122. Pedro R, Sardinha M, Reis L, et al. Ultrasonic fatigue testing in as-built and polished Ti6Al4V alloy manufactured by SLM. Forces Mech 2021;4:100024; doi: 10.1016/j.finmec.2021.100024 [DOI] [Google Scholar]
  • 123. Dareh A, Nafisi S, Hashemi R, et al. Experimental realisation of build orientation effects on the mechanical properties of truly as-built Ti-6Al-4V SLM parts. J Manuf Process 2021;64:140–152; doi: 10.1016/j.jmapro.2021.01.027 [DOI] [Google Scholar]
  • 124. Sanaei N, Fatemi A. Analysis of the effect of surface roughness on fatigue performance of powder bed fusion additive manufactured metals. Theor Appl Fract Mech 2020;108:102638; doi: 10.1016/j.tafmec.2020.102638 [DOI] [Google Scholar]
  • 125. Li J, Hu J, Zhu Y, et al. Surface roughness control of root analogue dental implants fabricated using selective laser melting. Addit Manuf 2020;34:101283; doi: 10.1016/j.addma.2020.101283 [DOI] [Google Scholar]
  • 126. Yánez A, Paula M, Cuadrado A, et al. Surface roughness effects on the fatigue behaviour of gyroid cellular structures obtained by additive manufacturing. Int J Fatigue 2020;138:105702; doi: 10.1016/j.ijfatigue.2020.105702 [DOI] [Google Scholar]
  • 127. Günther J, Leuders S, Koppa P, et al. On the effect of internal channels and surface roughness on the high-cycle fatigue performance of Ti-6Al-4V processed by SLM. Mater Des 2018;143:1–11; doi: 10.1016/j.matdes.2018.01.042 [DOI] [Google Scholar]
  • 128. Khorasani A, Gibson I, Sha U, et al. The effect of SLM process parameters on density, hardness, tensile strength and surface quality of Ti-6Al-4V. 2019;25:176–186; doi: 10.1016/j.addma.2018.09.002 [DOI] [Google Scholar]
  • 129. Lerebours A, Vigneron P, Bouvier S, et al. Additive manufacturing process creates local surface roughness modifications leading to variation in cell adhesion on multifaceted. Bioprinting 2019;16:e00054; doi: 10.1016/j.bprint.2019.e00054 [DOI] [Google Scholar]
  • 130. Fielden-Stewart Z, Coope T, Bacheva D, et al. Effect of the surface morphology of SLM printed aluminium on the interfacial fracture toughness of metal-composite hybrid joints. Int J Adhes Adhes 2021;105:102779; doi: 10.1016/j.ijadhadh.2020.102779 [DOI] [Google Scholar]
  • 131. Plessis A, Beretta S. Killer notches: The effect of as-built surface roughness on fatigue failure in AlSi10Mg produced by laser powder bed fusion. Addit Manuf 2020;35:101424; doi: 10.1016/j.addma.2020.101424 [DOI] [Google Scholar]
  • 132. Mohammadi M, Asgari H. Achieving low surface roughness AlSi10Mg_200C parts using direct metal laser sintering. Addit Manuf 2018;20:23–32; doi: 10.1016/j.addma.2017.12.012 [DOI] [Google Scholar]
  • 133. Maamoun AH, Xue YF, Elbestawi MA, et al. Effect of selective laser melting process parameters on the quality of al alloy parts: Powder characterization, density, surface roughness, and dimensional accuracy. Materials (Basel) 2018;11(12):2343; doi: 10.3390/ma11122343 [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 134. Seltzman AH, Wukitch SJ. Surface roughness and finishing techniques in selective laser melted GRCop-84 copper for an additive manufactured lower hybrid current drive launcher. Fusion Eng Des 2020;160:111801; doi: 10.1016/j.fusengdes.2020.111801 [DOI] [Google Scholar]
  • 135. Favero G, Bonesso M, Rebesan P, et al. Additive manufacturing for thermal management applications: From experimental results to numerical modeling. Int J Thermofluids 2021;10:100091; doi: 10.1016/j.ijft.2021.100091 [DOI] [Google Scholar]
  • 136. Nicoletto G, Kone R, Frká M, et al. Surface roughness and directional fatigue behavior of as-built EBM and DMLS Ti6Al4V. Int J Fatigue 2018;116:140–148; doi: 10.1016/j.ijfatigue.2018.06.011 [DOI] [Google Scholar]
  • 137. Ramanathan A, Moverare J, Dixit N, et al. Influence of defects and as-built surface roughness on fatigue properties of additively manufactured Alloy 718. Mater Sci Eng A 2018;735:463–474; doi: 10.1016/j.msea.2018.08.072 [DOI] [Google Scholar]
  • 138. Akgun E, Zhang X, Biswal R, et al. Fatigue of wire+arc additive manufactured Ti-6Al-4V in presence of process-induced porosity defects. Int J Fatigue 2021;150:106315; doi: 10.1016/j.ijfatigue.2021.106315 [DOI] [Google Scholar]
  • 139. Aldalur E, Suárez A, Veiga F. Metal transfer modes for wire arc additive manufacturing Al-Mg alloys: Influence of heat input in microstructure and porosity. J Mater Process Technol 2021;297:117271; doi: 10.1016/j.jmatprotec.2021.117271 [DOI] [Google Scholar]
  • 140. Fu R, Tang S, Lu J, et al. Hot-wire arc additive manufacturing of aluminum alloy with reduced porosity and high deposition rate. Mater Des 2021;199:109370; doi: 10.1016/j.matdes.2020.109370 [DOI] [Google Scholar]
  • 141. Wang J, Zhu K, Zhang W, et al. Microstructural and defect evolution during WAAM resulting in mechanical property differences for AA5356 component. J Mater Res Technol 2022;22:982–996; doi: 10.1016/j.jmrt.2022.11.116 [DOI] [Google Scholar]
  • 142. Rajkumar V, Vishnukumar M, Sowrirajan M, et al. Microstructure, mechanical properties and corrosion behaviour of Incoloy 825 manufactured using wire arc additive manufacturing. Vacuum 2022;203:111324; doi: 10.1016/j.vacuum.2022.111324 [DOI] [Google Scholar]
  • 143. Vishnukumar M, Pramod R, Rajesh Kannan A. Wire arc additive manufacturing for repairing aluminium structures in marine applications. Mater Lett 2021;299:130112; doi: 10.1016/j.matlet.2021.130112 [DOI] [Google Scholar]
  • 144. Kokare S, Oliveira JP, Santos TG, et al. Environmental and economic assessment of a steel wall fabricated by wire-based directed energy deposition. Addit Manuf 2023;61:103316; doi: 10.1016/j.addma.2022.103316 [DOI] [Google Scholar]
  • 145. Vessels OP, Bars SS, Castings RA, et al. Standard specification for additive manufacturing stainless steel alloy (UNS S31603) with powder bed fusion 1. N.d.;i:1–9; doi: 10.1520/F3184. [DOI] [Google Scholar]
  • 146. ASTM F3413-19e1. Guide for Additive Manufacturing—Design—Directed Energy Deposition. ASTM Int 2022; 2022:1–24; doi: 10.1520/F3413-19E01 [DOI] [Google Scholar]
  • 147. ASTM, ISO. 52901:2016(E): Standard guide for additive manufacturing—General principles—Requirements for purchased AM parts 1. 2019;2016:1–7. [Google Scholar]
  • 148. ASTM International. Additive manufacturing—Design—Part 1: Laser-based powder bed fusion of metals 1. ASTM Int 2019;2019:1–15; doi: 10.1520/52911-1-19.2 [DOI] [Google Scholar]
  • 149. ASTM, ISO. 52911-3:2023: Additive manufacturing–Design–Part 3: PBF-EB of metallic materials: 2023;2023:1–26. [Google Scholar]
  • 150. ASTM 52900. Additive manufacturing—General principles—Terminology. ASTM Int 2021;2021:1–14. [Google Scholar]
  • 151. ASTM International. Standard specification for additive manufacturing nickel alloy (UNS N07718) with powder bed fusion (F3055-14a). 2021;14(Reapproved):1–8; doi: 10.1520/F3056-14R21.Copyright [DOI] [Google Scholar]
  • 152. Bang GB, Park JH, Kim WR, et al. Study on the effect of preheating temperature of SLM process on characteristics of CoCrMo alloy. Mater Sci Eng A 2022;841:143020; doi: 10.1016/j.msea.2022.143020 [DOI] [Google Scholar]
  • 153. Nudelis N, Mayr P. A novel classification method for pores in laser powder bed fusion. Metals (Basel) 2021;11(12):1–16; doi: 10.3390/met11121912 [DOI] [Google Scholar]
  • 154. Irrinki H, Nath SD, Akilan AA, et al. Laser powder bed fusion. Addit Manuf Process 2020;24:209–219; doi: 10.31399/asm.hb.v24.a0006621 [DOI] [Google Scholar]
  • 155. Mahamood RM, Akinlabi ET, Shukla M, et al. Characterizing the Effect of Processing Parameters on the Porosity of Laser Deposited Titanium Alloy Powder. In: Proceedings of the International MultiConference of Engineers and Computer Scientists, March 12–14, 2014, Hong Kong; 2014, Vol II4. [Google Scholar]
  • 156. Susan DF, Puskar JD, Brooks JA, et al. Quantitative characterization of porosity in stainless steel LENS powders and deposits. Mater Charact 2006;57(1):36–43. [Google Scholar]
  • 157. Ning F, Hu Y, Liu Z, et al. Ultrasonic vibration-assisted laser engineered net shaping of Inconel 718 parts: A feasibility study. Proc Manuf 2017;10:771–778. [Google Scholar]
  • 158. Khairallah SA, Anderson AT, Rubenchik A, et al. Laser powder-bed fusion additive manufacturing: Physics of complex melt flow and formation mechanisms of pores, spatter, and denudation zones. Acta Mater 2016;108:36–45. [Google Scholar]
  • 159. Thijs L, Verhaeghe F, Craeghs T, et al. A study of the microstructural evolution during selective laser melting of Ti–6Al–4V. Acta Mater 2010;58(9):3303–3312; doi: 10.1016/j.actamat.2010.02.004 [DOI] [Google Scholar]
  • 160. Courtois M, Carin M, Le Masson P, et al. A new approach to compute multi-reflections of laser beam in a keyhole for heat transfer and fluid flow modelling in laser welding. J Phys D Appl Phys 2013;46(50):505305. [Google Scholar]
  • 161. Cao L. Mesoscopic-scale simulation of pore evolution during laser powder bed fusion process. Comput Mater Sci 2020;179:109686. [Google Scholar]
  • 162. Zheng H, Li H, Lang L, et al. Effects of scan speed on vapor plume behavior and spatter generation in laser powder bed fusion additive manufacturing. J Manuf Process 2018;36:60–67; doi: 10.1016/j.jmapro.2018.09.011 [DOI] [Google Scholar]
  • 163. Ly S, Rubenchik AM, Khairallah SA, et al. Metal vapor micro-jet controls material redistribution in laser powder bed fusion additive manufacturing. Sci Rep 2017;7(1):1–12. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 164. Lin R, Wang H, Lu F, et al. Numerical study of keyhole dynamics and keyhole-induced porosity formation in remote laser welding of Al alloys. Int J Heat Mass Transf 2017;108:244–256; doi: 10.1016/j.ijheatmasstransfer.2016.12.019 [DOI] [Google Scholar]
  • 165. Panwisawas C, Perumal B, Ward RM, et al. Keyhole formation and thermal fluid flow-induced porosity during laser fusion welding in titanium alloys: Experimental and modelling. Acta Mater 2017;126:251–263. [Google Scholar]
  • 166. Shrestha S, Chou K. A study of transient and steady-state regions from single-track deposition in laser powder bed fusion. J Manuf Process 2021;61:226–235. [Google Scholar]
  • 167. Gong H, Rafi K, Gu H, et al. Influence of defects on mechanical properties of Ti—6Al—4 V components produced by selective laser melting and electron beam melting. Mater Des 2015;86:545–554. [Google Scholar]
  • 168. Watring DS, Carter KC, Crouse D, et al. Mechanisms driving high-cycle fatigue life of as-built Inconel 718 processed by laser powder bed fusion. Mater Sci Eng A 2019;761:137993; doi: 10.1016/j.msea.2019.06.003 [DOI] [Google Scholar]
  • 169. Mutke C, Geenen K, Röttger A, et al. Interaction between laser radiation and metallic powder of 316L austenitic steel during selective laser melting. Mater Charact 2018;145:337–346. [Google Scholar]
  • 170. Li C, Liu ZY, Fang XY, et al. Residual stress in metal additive manufacturing. Proc CIRP 2018;71:348–353. [Google Scholar]

Associated Data

This section collects any data citations, data availability statements, or supplementary materials included in this article.

Data Availability Statement

No data were used for the research described in the article.


Articles from 3D Printing and Additive Manufacturing are provided here courtesy of SAGE Publications

RESOURCES