Skip to main content
Heliyon logoLink to Heliyon
. 2024 Sep 26;10(19):e38425. doi: 10.1016/j.heliyon.2024.e38425

Synthesis of a new quaternary ammonium salt for efficient inhibition of mild steel corrosion in 15 % HCl: Experimental and theoretical studies

Lipiar KMO Goni a, Shaikh A Ali a,b, Hasan A Al-Muallem a,c, Mohammad A Jafar Mazumder a,b,⁎
PMCID: PMC11482660  PMID: 39416823

Abstract

The corrosion phenomenon and its economic impacts can hardly be ignored in any application. This study synthesized a quaternary ammonium salt (3) containing hydrophobic dodecyl and electron-rich diallylbenzyl amine moieties to be used in 15 % HCl as a corrosion inhibitor of mild steel. Several techniques, such as 1H and 13C NMR, IR, TGA, and elemental analysis, have been used to characterize inhibitor 3. Popular corrosion measurement techniques, namely weight loss, potentiodynamic polarization techniques, and electrochemical impedance spectroscopy, have been used to determine the efficiency of inhibitor 3. At 303 K and a moderately low concentration of 50 ppm, the quaternary ammonium salt-based inhibitor demonstrated a maximum efficiency of ≈95.0 %. At elevated temperatures of 313, 323, and 333 K, the inhibition efficacy values were recorded as 91.3, 82.8, and 75.0 %, respectively. Adsorption isotherm study revealed that the adsorption of inhibitor 3 followed Langmuir adsorption isotherm. The value of ΔGads° was found to be – 40.19 kJ mol−1, indicating that inhibitor 3 became adsorbed via a mixed physi-chemisorption mechanism. A very high adsorption constant (Kads) of 1.53 × 105 L mol−1 suggested strong adsorption of inhibitor 3. The difference in activation energy (Ea) value of 42.4 kJ mol−1 between the control and the inhibited solution indicated an efficient adsorption of inhibitor 3. The ability of inhibitor 3 to retard both anodic and cathodic half-cell reactions was proved via open circuit potential and Tafel curves studies. Detailed discussions on the change in corrosion current densities (icorr), polarization (Rp) and charge transfer (Rct) resistances have been offered to discuss the inhibition efficiency. Water contact angle measurement showed a drastic increase in mild steel surface hydrophobicity following inhibitor 3 adsorption. SEM-EDX and XPS studies confirmed the definitive presence of inhibitor 3 on the mild steel surface. Density functional theory (DFT) studies revealed the frontier molecular orbitals with which the metal surface interacts. A detailed corrosion inhibition mechanism has been offered in the context of adsorption isotherm and DFT studies.

Keywords: Quaternary ammonium salt, 15 % HCl, Mild steel, Corrosion inhibition, Inhibitor adsorption, Acidizing corrosion

Graphical abstract

Image 1

Highlights

  • •

    A new quaternary ammonium salt compound was synthesized as a mild steel corrosion inhibitor.

  • •

    A very high inhibition efficiency of 95.2 % was measured under acidizing conditions (15 % HCl).

  • •

    The proposed inhibitor was successfully tested at different temperatures (303–333 K).

  • •

    Quaternary ammonium salt having a hydrophobic long-chain alkyl group boosts inhibition efficiency.

  • •

    The frontier molecular orbitals of the inhibitor disclosed the sights that interact with the metal surface.

1. Introduction

Corrosion is an electrochemical process that causes the metal to degrade when it's in contact with a corrosive medium, forcing it to undergo mass and charge transfer simultaneously [1]. The menaces of corrosion are so pervasive that corrosion-related costs account for ≈5–7 % of any nation's GNP [2]. Owing to strength and affordability, low-carbon steel, containing carbon in the range of 0.05–0.3 %, has seen myriad applications for industrial and engineering purposes [3]. In oil and gas industries, acidizing technology is very crucial to increasing oil and gas production. Generally, concentrated acids, 15–28 % HCl in general, are flushed into the reservoir through the wellbore, and these acids crush the clay minerals and carbonate rocks. This causes the reservoir permeability to increase and the flow paths to improve, thereby enhancing oil recovery [4]. Unfortunately, because they are highly corrosive, acids cause severe damage to downhole metallic equipment, resulting in economic losses of various magnitudes.

A recent study by the NACE demonstrated that the global cost of corrosion equated to 3.4 % of the worldwide GDP in 2013 [5]. The current corrosion cost can be reduced by 15–35 %, equating to 375–875 US billion dollars, using the available anticorrosion methods [6]. One prevalent, economical, and easy-to-use approach is corrosion inhibitors [7]. Corrosion inhibitors, as the name implies, are chemical compounds that, when added/used in meager concentrations, can significantly reduce the metal dissolution rate. Small molecules or organic compounds are widely used to mitigate the corrosion of steels in acidic media [8]. Organic compounds contain different functionalities and experience chemical/electrostatic interactions or a combination of both with the metal surface in solution. Therefore, these molecules having N, O, S, and P heteroatoms, aromatic rings, π-systems, conjugated bonds, polar functional groups (–NO2, –NH2, –COOH, –OH, –CN, –C=O), etc., are considered effective corrosion inhibitors.

Quaternary ammonium compounds effectively counter the corrosion of metals and other underground pipelines in acidic media [9,10]. The quaternary ammonium moiety is advantageous and can be decorated with different functionalities to tailor and improve the inhibition efficiency. Moreover, different alkyl chain lengths and hydrophobic motifs can be incorporated into quaternary ammonium compounds, which have proven useful [11,12]. To counter the corrosion of carbon steel in 1 M HCl, Chauhan et al. [13] studied the anticorrosion properties of a tripropylamine-based quaternary salt. At a high concentration of 200 ppm, the inhibitor showed a maximum inhibition efficiency (IE) of 93 %. A quaternary ammonium salt surfactant corrosion inhibitor was used by Jalab et al. [14] to study the corrosion of carbon steel in 5 M HCl. At a concentration of 2.22 mM, the inhibitor achieved a low IE of 56.0 %. To inhibit mild steel corrosion in 1 M HCl, Haque et al. [11] studied the IE of three propargyl pyrrolidium bromide quaternary ammonium salts (DPPB, DDPPB, and HDPPB). For a small concentration of 60.3 μM, DPPB, DDPPB, and HDPPB showed excellent IEs of 92.6, 93.7, and 96.2 %, respectively. Tabei et al. [15] used a bis-cationic surfactant to retard carbon steel corrosion in 1 M HCl. It was found to inhibit the corrosion of carbon steel by 94.7 % at a concentration of 1 × 10−3 M. The anti-corrosive effects of dodecyl trimethyl ammonium bromide and thiourea mixture (DTAB-Thiourea) and dodecyl dimethyl benzyl ammonium bromide (DDBAB-Thiourea) were studied for Q235 steel corrosion in 0.05 mol L−1 [16]. DTAB-Thiourea and DDBAB-Thiourea inhibited the corrosion of Q235 steel by 93.37 and 94.98 %, respectively.

Mild steel has seen tremendous applications because of its extraordinary mechanical strength, easy availability, and low cost. It is extensively used across many industries for fabrication and construction. However, when subjected to different organic and inorganic acids during chemical or electrochemical processes in oil refineries and shipbuilding, as well as during acid cleaning, pickling, and metals descaling, mild steel suffers from severe corrosion [17,18]. Therefore, it's imperative that new corrosion inhibitors must be synthesized to be used in extremely harsh acid conditions. In this study, we synthesized a new quaternary ammonium chloride salt (3) (Scheme 1) containing a diallyl amine moiety with unquenched nitrogen, a benzene ring with π-electrons, and a favorable alkyl chain length to promote hydrophobicity on the mild steel surface. To the best of our knowledge, this is the first instance of this compound being reported. The proposed inhibitor has a good balance of hydrophobicity in the form of an alkyl chain moiety and hydrophilicity in the form of a quaternary ammonium salt moiety. As such, the inhibitor demonstrated an excellent IE tested via several corrosion measuring techniques. A very high inhibition efficiency of 95.2 % was registered for just 0.1 mM inhibitor concentration, which is rare in literature (vide infra, see Table 7). Following very efficient adsorption of inhibitor 3, several surface characterization techniques were employed to prove the adsorption of inhibitor 3. DFT-based computational studies have also been performed to develop knowledge of the inhibitor sites that establish chemical communication with the metal surface.

Scheme 1.

Scheme 1

Synthesis of inhibitor molecule 3.

Table 7.

Some recently reported surfactant corrosion inhibitors of steels in acid media.

Inhibitor Concentration Metal/Electrolyte (Temperature) Inhibition efficiency (%) References
Image 1 (DBBD) 20 mM Mild steel/15 % HCl (25 °C) 98.0 [66]
Image 2 (MCS-14) 1 mM API X65/3 M HCl (25 °C) 93.1 [67]
Image 3 (12-MOH-O-MOH-12) 3 mM AISI 304 SS/3 M HCl (25 °C) 98.0 [68]
Image 4 (PMTH2E8) 4.2 mM AISI 304 SS/3 M HCl (25 °C) 98.0 [69]
Image 5 (TMTN12Br) 3 mM AISI 304 SS/3 M HCl (25 °C) 98.0 [70]
Image 6 (QAS-12) 0.5 mM Q235 MS/15 % HCl (30 °C) 93.1 [71]
Image 7 (DMAEB) 100 ppm N80 CS/15 % HCl (30 °C) 96.8 [72]
Image 8 (CGS) 200 ppm LCS/15 % HCl (25 °C) 94.7 [73]
Image 9(Q8Q) 13 mM N80 steel/15 % HCl (25 °C) 95.5 [74]
Image 10 (Inhibitor 3) 50 ppm (0.1 mM) Mild steel/15 % HCl (30 °C) 95.2 This work

2. Experimental

2.1. Materials

The quaternary ammonium compound (1) was synthesized following a work reported earlier [19]. Diallylamine (2) was acquired from Sigma-Aldrich and used as obtained. The metal samples (mild steel specimens) were obtained from Chrome Royal Al Arabian Contracting Ltd, Riyadh, Saudi Arabia, as a gift. All the solvents (analytical grade) required for this study were bought from Sigma-Aldrich and used as they arrived. The used mild steel samples were of the composition (wt.%): C (0.21 %), P (0.06 %), Si (0.29 %), Cu (0.06 %), S (0.05 %), Mn (0.49 %), and Fe (balance). The corrosive medium (the electrolyte test solution) was 15 % HCl, prepared by diluting 37 % HCl with deionized water.

2.2. Physical methods

A PerkinElmer (2400 Series II) CHNS/O elemental analyzer was used to find out the atomic compositions of inhibitor 3. A PerkinElmer 16 PC FTIR spectrometer was used to record the IR spectra. CDCl3 was used as the solvent to record 1H and 13C NMR spectra using a 400-MHz Bruker Avance III spectrometer. TMS and 13C CDCl3 signals at δ 0 and 77.0 ppm were used as references, respectively. Thermogravimetric analysis (TGA) of 3 was carried out using SDT Q600 developed by the TA Instruments. Thermal stability of 3 was conducted under N2 flow (50 mL min−1) condition. The TGA curves were recorded from 20 °C until 800 °C, increasing the temperature by 10 °C per minute.

2.3. Synthesis of inhibitor molecule 3

The synthesis route for preparing inhibitor molecule 3 is presented as Scheme 1. Briefly, in 25 mL acetonitrile, a solution of 1 (3.88 g, 10.0 mmol) and 2 (4.86 g, 50 mmol) was stirred under N2 at 65 °C for 24 h. Following the removal of the solvent and remaining diallyl amine 2, 20 mL of deionized water was used to dissolve the remainder of the mixture, followed by treating with NaOH (500 mg, 12.5 mmol). Afterward, the aqueous layer was extracted with three portions (50 mL each) of diethyl ether. A saturated NaCl solution (20 mL) was used to wash the organic layer before drying it over Na2SO4. Diethyl ether was removed, and the residue was dried under vacuum at 60 °C, which afforded inhibitor compound 3 as a light-yellow semisolid (4.27 g, 95 %).

2.4. Corrosion studies

2.4.1. Gravimetric weight loss

To conduct the gravimetric WL tests, mild steel coupons (2.8 cm × 2.8 cm × 0.6 cm) were prepared and cleaned following ASTM standards (ASTM G31-21). After taking their weight, mild steel coupons were immersed in 15 % HCl solution with and without inhibitors in 250 mL Wheaton bottles filled up to 200 mL. The coupons were allowed to corrode in the absence and presence of 3 (1, 5, 10, 20, 50, and 100 ppm) for 3 h at 30 °C (303 K). The weight loss tests at each temperature were triplicated, and the mean value was used to calculate the IEs. After 3 h, the coupons were taken out of the bottles. The corrosion products on the coupons were cleaned following the ASTM mentioned above standards. After that, the final weight of the coupons was measured after they were dried. To facilitate thermodynamics studies, additional WL tests were conducted at 313, 323, and 333 K. Eq. (1) was used to calculate the IEs imparted by different concentrations of 3 and Eq. (2) to calculate the corrosion rates (CR).

ηWL(%)=Wo−WiWo×100 (1)
CR(mmy−1)=87.6×ΔWDAT (2)

Where, Wo and Wi represent weight losses in the absence and presence, respectively, of inhibitor 3, ΔW = Wb−Wa, where Wb and Wa depict the weight of mild steel coupons before and after immersion, respectively, D is the density of Fe in mild steel (7.87 g cm−3), A is the exposed coupon area, and T is the immersion time (3 h). The area of the metal coupons was calculated using the formula: 2[(length × width)+(width × height)+(height × length)], with the dimensions being measured in cm.

2.4.2. Electrochemical corrosion study

The electrochemical studies were conducted using a Gamry three-electrode electrochemical cell in a static condition at 30 °C. A graphite rod, a piece of mild steel, and a standard calomel electrode (SCE) were used as the counter, working, and reference electrodes. The electrochemical cell can accommodate 300 mL testing solutions and is designed to expose only a 1 cm2 working electrode (mild steel) area to the testing solutions. A Gamry Reference 3000 Potentiostat/Galvanostat/ZRA was used to conduct electrochemical corrosion studies, and the electrochemical cell was connected to it. The Gamry framework system (ESA410) associated with the Gamry Reference 3000 was utilized to record the impedance and polarization curves. The recorded curves were fitted using Echem Analyst software (version: 7.8.2) developed by Gamry to derive relevant electrochemical parameters. Before each measurement, the open circuit potential (EOCP) was recorded for 1 h to allow the system to gain a stable potential. EIS measurements were carried out in the 10 kHz to 10 mHz frequency range using a small, 10 mV AC perturbation. The IEs from EIS measurements (ηEIS%) were calculated using Eqs. (3), (4).

ηEIS(%)=(1−Rct°RT)×100 (3)
RT=Rct+Rfm (4)

Where, Rct° and Rct represent charge transfer resistance in the absence and presence of the inhibitor, respectively, Rfm means the film resistance arising from the adsorption of the inhibitor and RT stands for total resistance.

At a scan rate of 0.5 mV/s, the mild steel surface was polarized by ±250 mV against the EOCP value to record the PDP curves. The Tafel region of the PDP curves were used to extrapolate all electrochemical parameters. At a scan rate of 0.125 mV/s, the mild steel surface was polarized by ±10 mV against the EOCP to record the LPR curves. Polarization resistance values (Rp) were recorded by selecting two points on the LPR curves, keeping the zero current value roughly in the middle. The IEs values from the PDP and LPR techniques, ηPDP(%) and ηLPR(%), respectively, were calculated using Eqs. (5), (6).

ηPDP(%)=(1−icorricorr°)×100 (5)
ηLPR(%)=(1−Rp°Rp)×100 (6)

Where, icorr° and icorr denote corrosion current densities in the absence and presence of the inhibitor, respectively, and Rp° and Rp represent polarization resistances in the absence and presence of the inhibitor, respectively.

2.5. Surface studies

Mild steel coupons with smaller dimensions (1 cm × 1 cm × 0.3 cm) were used for surface evaluation. The coupons were thoroughly abraded with SiC papers of different grit sizes (#120 – #1200), followed by rinsing with acetone to remove moisture and drying in warm air before carrying out the immersion tests. The concentration of inhibitor 3 used for surface analyses was 50 ppm. After completing the immersion tests, which continued for 3 h, the coupons were taken out, dried in a cold stream of air, and submitted for analysis. Scanning electron microscopy (SEM) analyses were carried out using Quattro ESEM – FEG (Thermo Fisher Scientific) coupled with an EDX (Oxford Instruments). X-ray photoelectron spectroscopy (XPS) studies that revealed the bound state of the adsorbed elements were carried out by a Thermo Fisher Scientific ESCALAB 250Xi XPS microprobe. The microprobe could produce monochromatic Al Kα X-ray radiations with photon energy 1486.7 eV and wavelength 8.3386 Å. The spot size and base pressure were maintained at 650 μm and 10−10 mbar, respectively. Avantage (version: 5.51) software was used to deconvolute the XPS spectra and fit the peaks. Water contact angle measurements were carried out using the KRŰSS Drop Shape Analyzer (DSA30E). The volume of each drop was maintained at 2 μL and formed at a rate of 2.67 μL/s. The analysis was performed using the sessile drop orientation and ellipse fitting method.

2.6. Density functional theory

Density functional theory (DFT)-based quantum chemical calculations were performed using a very popular DFT functional called B3LYP. The calculations were performed using Gaussian 09, and the basis set selected for this purpose was 6-31G+(d,p) [20]. The electronic properties associated with the corrosion inhibitor dictate how good the inhibitor is [21]. Different reactivity parameters derived from the frontier molecular orbitals (FMOs) energies were calculated using Eqs. (10), (11), (12), (13), (7), (8), (9):

ΔE=ELUMO−EHOMO (7)
IP=−EHOMO (8)
EA=−ELUMO (9)
η=12(ELUMO−EHOMO) (10)
σ=1η (11)
χ=−12(ELUMO+EHOMO) (12)
ΔN=χFe−χinh2(ηFe+ηinh) (13)

Where, ΔE stands for HOMO–LUMO gap, IP represents ionization potential, and EA means electron affinity. On the other hand, η and σ represent global hardness and global softness, respectively. χ represents electronegativity, and ΔN indicates the fraction of electron transfer.

3. Results and discussion

3.1. Characterization of quaternary ammonium salt inhibitor (3)

The comprehensive elemental analysis of the inhibitor molecule 3, with the molecular formula C28H49ClN2 (MW; 449.16 g mol−1), FTIR, 1H, and 13C Nuclear magnetic resonance (NMR) spectra, and thermogravimetry analysis (TGA), is presented below.

The elemental analysis of inhibitor molecule 3, with the molecular formula C28H49ClN2 (MW; 449.16 g mol−1), found C 74.3, H 11.3, and N 5.9 %. C28H49ClN2 requires C 74.87; H 11.00; N 6.24 %). νmax (KBr): 3451 (moisture), 3077, 3008, 2922, 2853, 2808, 2708, 1842, 1642, 1617, 1514, 1485, 1468, 1418, 1368, 1258, 1220, 1149, 1119, 1074, 996, 919, 872, 818, 760, 722, 642, 561, and 465 cm−1 (see supplementary information, Fig. S1).

δH (CDCl3) 0.88 (3H, t, J 7.2 Hz), 1.10–1.35 (18 H, m), 1.72 (2H, m), 2.17 (moisture, br), 3.07 (4H, d, J 6.4 Hz) 3.31 (6H, s), 3.46 (2H, m), 3.59 (2H, s), 4.97 (2H, s), 5.17 (4H, m), 5.86 (2H, m), 7.43 (2H, d, J 7.8 Hz), 7.56 (2H, d, J 7.8 Hz); δC (CDCl3) 13.93 (1C), 22.47 (1C), 22.73 (1C), 26.13 (1C), 29.07 (1C), 29.11 (1C), 29.18 (1C), 29.24 (2C), 29.37 (1C), 31.69 (1C), 49.40 (2C), 56.36 (2C), 56.76 (1C), 63.19 (1C), 66.94 (1C), 117.45 (2C), 125.72 (1C), 129.13 (2C), 132.90 (2C), 135.33 (2C), 142.53 (1C). (CDCl3 middle C:77.00).

The 1H and 13C NMR spectra of inhibitor molecule 3 with the relevant assignments are depicted in Fig. 1.

Fig. 1.

Fig. 1

(a) 1H and (b) 13C NMR spectrum of inhibitor molecule 3 in CDCl3.

As shown in Fig. S2, the TGA curve depicts the thermal stability of the inhibitor molecule 3 is up to ≈200 °C.

3.2. Gravimetric studies

3.2.1. Effect of concentration and temperature

To understand the effect of inhibitor 3 on the corrosion of mild steel in 15 % HCl, gravimetric WL studies were carried out for different concentrations of inhibitor 3 at 30 °C. Table 1 shows the extent of WL occurred in the absence and presence of 1, 5, 10, 20, 50, and 100 ppm of inhibitor 3. In the absence of inhibitor 3, highly corrosive 15 % HCl caused the mild steel coupon to experience a WL of 224.4 mg. The WL was found to be a little less following the immersion of mild steel in 1 ppm inhibitor 3 solution. However, CR values started declining significantly starting from the concentration of 5 ppm and onwards. Whereas 1 ppm of inhibitor 3 imparted a low IE of 4.1 %, it improved to 53.2 % in the presence of 5 ppm. After that, with increasing concentrations, the IE started increasing, and CR values kept declining. At 10, 20, 50, and 100 ppm of 3, the IE values were calculated to be 77.1, 88.4, 94.2, and 94.5 %, respectively. In the absence of inhibitor 3, CR was found to be 33.7 mmy−1, which declined radically to 2 mmy−1 in the presence of 50 ppm of the inhibitor. Fig. 2a shows the variation in IE and CR values with the change in inhibitor concentration. A corrosion inhibitor is suitable for a specific electrolyte medium if the IE imparted by it is higher than 90 % at concentrations of tens or hundreds of ppm [22]. Inhibitor 3 reached a maximum IE of 94.2 % at only 50 ppm. The inhibitor molecule contains certain functionalities designed to help it adsorb better on the metal surface. The presence of a lone pair of electrons on nitrogen, π-electrons in the benzene ring, quaternary ammonium moiety, and chloride counter ions made physical and/or chemical interactions with the metal surface that are positively charged.

Table 1.

Weight loss study data for the corrosion of mild steel in the presence and absence of inhibitor 3 in 15 % HCl at different temperatures.

Temp (°C) Conc. (ppm) Weight loss (mg)a CR (mm y−1)a Surface coverage (θ) ηWL (%)a
30
Blank 224.4 ± 0.70 33.7 ± 0.11 – –
1 215.2 ± 0.44 32.3 ± 0.07 0.041 4.1 ± 0.43
5 105 ± 0.56 15.8 ± 0.08 0.532 53.2 ± 0.14
10 51.4 ± 0.46 7.7 ± 0.07 0.771 77.1 ± 0.24
20 26 ± 0.66 3.9 ± 0.10 0.884 88.4 ± 0.26
50 13 ± 1.01 2 ± 0.15 0.942 94.2 ± 0.44
100
12.3 ± 0.26
1.9 ± 0.04
0.945
94.5 ± 0.11
40
Blank 499.8 ± 0.26 75.1 ± 0.04 – –
50
43.3 ± 0.20
6.5 ± 0.03
0.913
91.3 ± 0.04
50
Blank 1099.1 ± 1.15 165.2 ± 0.17 – –
50
188.9 ± 0.96
28.4 ± 0.14
0.828
82.8 ± 0.10
60 Blank 2278.5 ± 0.46 342.4 ± 0.07 – –
50 568.6 ± 0.61 85.5 ± 0.09 0.750 75.0 ± 0.03
a

The numerical values after ‘±’ represent the standard deviation.

Fig. 2.

Fig. 2

Change in IE and CR values for mild steel corrosion in the presence of inhibitor 3 at 30 °C (a) and 50 ppm of 3 at different temperatures (b).

Additionally, an alkyl chain length in the inhibitor molecule certainly contributed to a surge in hydrophobicity on the metal surface that neutralized the aggression of corrosive water molecules [23]. However, the IE didn't experience any further increase after 50 ppm, as the IE values imparted by 50 and 100 ppm of inhibitor 3 are almost the same. This indicates that the adsorption sites on the metal surface are all occupied by the inhibitor molecules present at the concentration of 50 ppm. Therefore, increasing the concentration after that doesn't help anymore. Thus, 50 ppm of inhibitor 3 is the optimum concentration to achieve the best performance.

As inhibitor 3 showed the maximum IE at 50 ppm, this concentration was chosen for surface studies and observing the effect of temperatures that would reveal valuable thermodynamic parameters (vide infra, section 3.2.3). Table 1 and Fig. 2b show the variation in IE and CR values as mild steel coupons are tested in the presence and absence of 50 ppm of inhibitor 3 at different temperatures. At 40 °C, the IE was found to be 91.3 %, which is still very close to that obtained at 30 °C. At 50 °C and 60 °C, the IE values declined to 82.8 and 75.0 %, respectively. The IE of an inhibitor decreasing with increasing temperature can be linked to its adsorption via the physisorption/electrostatic interaction process, and this interaction gets weaker owing to thermal agitation [24]. Consequently, the CR values at 40, 50, and 60 °C were found to be 6.5, 28.4, and 85.5 mmy−1, respectively, increasing from 2 mmy−1 at 30 °C.

3.2.2. Adsorption isotherm

The WL data obtained from corrosion of mild steel in the presence of 3 at 30 °C was used to fit several adsorption isotherms (Eq. (14) – (17)). Fig. S3 shows different adsorption isotherm curves, and Table 2 outlines the relevant isotherm parameters obtained from isotherm fittings. The Langmuir isotherm represents the best fit (Eq. (15)). The correlation of coefficient value (R2) for Langmuir adsorption isotherm was found to be the closest to unity, indicating a much better fitting than R2 values of 0.8073, 0.8953, and 0.7590 obtained for Temkin, Frumkin, and Freundlich adsorption isotherms, respectively. Fig. S3a shows that the slope value obtained for Langmuir isotherm fitting is 1.0228, which is very close to 1. This indicates that the adsorption of inhibitor 3 on a mild steel surface follows the monolayer adsorption model [25]. Kads was calculated from the intercept of Langmuir adsorption isotherm and was found to have a very large value of 1.53 × 105 L mol−1, indicating a strong attractive force between inhibitor 3 and the metal surface. While the nature of Gibbs free energy value (ΔGads°) discloses the spontaneity of the adsorption process; its magnitude reveals the type of adsorption process adopted by the inhibitor. ΔGads° value for Langmuir adsorption isotherm was calculated following Eq. (18) and found to be – 40.19 kJ mol−1, as enumerated in Table 2. The negative value of ΔGads° proves that the adsorption of 3 on a mild steel surface is spontaneous. Generally, while ΔGads° value of – 20 kJ mol−1 or less negative indicates an electrostatic interaction between the inhibitor and the metal surface, and a value of – 40 kJ mol−1 or more negative suggests that electrons transfer the inhibitor to the metal surface [26]. Therefore, the calculated ΔGads° value of – 40.19 kJ mol−1 for the adsorption of inhibitor 3 suggests a mixed interplay between these two adsorption modes.

Freundlich:logθ=nlogC+logKads (14)
Langmuir:Cθ=C+1Kads (15)
Fumkin:θ=2.3032alogθ(1−θ)C−2.3032alogKads (16)
Temkin:θ=2.303flogC−2.303flogKads (17)
ΔGads°=−RTln(55.5×Kads) (18)

Where, θ represents surface coverage, C indicates inhibitor concentration (M), Kads is the adsorption constant, n, a, and f are Freundlich, Frumkin, and Temkin adsorbate characteristics, respectively. In Eq. (18), ΔGads° is the thermodynamic potential popularly known as Gibbs free energy, R is the universal gas constant having a value of 8.314 J mol−1 K−1, and T represents the absolute temperature in Kelvin, and 55.5 is the moles of water in 1 L of water.

Table 2.

Different isotherm parameters were obtained from WL studies carried out at 30 °C.

Temkin Frumkin Freundlich Langmuir
R2 f R2 a R2 n R2 Kads (L mol−1) ΔGads° (kJ mol−1)
0.8073 7.741 0.8953 7.108 0.7590 0.1744 0.9994 1.53 × 105 −40.19

3.2.3. Thermodynamic parameters

The study on the effect of temperature on CR (vide supra; section 3.2.1) was used to estimate the thermodynamic parameters, such as activation energy (Ea), enthalpy (ΔHads), and entropy (ΔSads) of adsorption. The slope of the plot log CR vs 1/T(K) was used to estimate Ea following Eq. (19) (Arrhenius equation). On the other hand, ΔHads and ΔSads were obtained from the slope and intercept, respectively, of the plot log CR/T vs. 1/T(K) following Eq. (20) (transition state equation).

logCR=logA−Ea2.303RT (19)
logCRT=[log(RNh)+(ΔSads2.303R)]−ΔHads2.303RT (20)

Where, A is the Arrhenius pre-exponential factor, R is the molar gas constant, N is Avogadros's constant, and h represents Planck's constant.

Arrhenius and transition state plots are represented by Fig. 3a and b, respectively. Several important thermodynamic parameters were obtained using these two plots. While the Ea value for the blank solution was calculated to be 65 kJ mol−1, the Ea value for 50 ppm-inhibited solution turned to be 107.4 kJ mol−1. The rise in the Ea value in the presence of inhibitor 3 indicates that the dissolution of the metal has become more difficult [[27], [28]]. In the absence and presence of inhibitor 3, the values of ΔHads were calculated to be 62.3 and 104.8 kJ mol−1, respectively. This means the adsorption of inhibitor 3 is endothermic in nature, and the mild steel dissolution lessens in the presence of the inhibitor [25]. The value of ΔSads, in the absence of inhibitor 3, was found to be −10.3 J mol−1 K−1. An increase in ΔSads from −10.3 J mol−1 K−1 to a very high value of 106.1 J mol−1 K−1 for the inhibitor adsorption indicates an increase in the disorder on the mild steel surface. This could be attributed to a faster displacement of the water molecules from the mild steel surface while the inhibitor molecules are adsorbed, providing better protection [29].

Fig. 3.

Fig. 3

log CR vs 1/T(K) (Arrhenius plot) (a) to calculate the Ea value and log CR/T vs. 1/T(K) (transition state plot) (b) providing ΔSads and ΔHads parameters for iron dissolution in the absence and presence of inhibitor 3 (50 ppm) at different temperatures (303–333 K).

3.3. Electrochemical corrosion studies

3.3.1. Open circuit potential (OCP)

Fig. 4a shows the potential-time curves (OCP curves) that were recorded after allowing the mild steel to corrode freely for 1 h at 30 °C in the absence and presence of different concentrations of inhibitor 3. These OCP curves show how, both in the presence and absence of the inhibitor, the electrical double layer on the metal surface adapts to the corrosive environment. The EOCP of the blank is shown to begin at around −510 mV vs. SCE and continues progressing in the anodic/(+ve) direction until a steady state is reached. This behavior can be explained as an attempt by the metal surface to develop a protective oxide layer following the corrosive attack of 15 % HCl solution [30]. An identical response could be observed when various amounts of inhibitor 3 are added to the harsh 15 % HCl solution. In the presence of 1, 5, 10, 20, 50, and 100 ppm of inhibitor 3, EOCP starts moving towards the (+ve) direction as the curve progresses. This suggests that inhibitor 3 functions by inspiring an anodic direction inhibition mechanism. However, since none of the EOCP shifts corresponding to different concentrations of 3 experienced a drift of more than 85 mV from that of the blank solution, the inhibition mechanism can be assumed to be of mixed–type, i.e., inhibitor 3 functions by retarding both anodic and cathodic half-cell reactions [31,32]. Importantly, as each OCP curve was observed to attain a steady state within 1 h, electrochemical measurements were able to be conducted under a stable system free of potential drift.

Fig. 4.

Fig. 4

OCP curves recorded for the corrosion of mild steel in the absence and presence of different concentrations of 3 in 15 % HCl for 1 h at 30 °C (a); EIS-mediated Nyquist plots (b) and Bode magnitude (along primary vertical axis) and phase angle (along secondary vertical axis) plots (c) recorded under the same conditions as OCP curves.

3.3.2. Electrochemical impedance spectroscopy (EIS)

The nature of the newly constructed electrical double layer (EDL) following OCP stabilization was evaluated in terms of EIS measurements represented by Nyquist plot (Fig. 4b), Bode magnitude (along the primary vertical axis), and Bode phase angle (along the secondary vertical axis) plots (Fig. 4c) in 15 % HCl with varying inhibitor 3 doses present and absent. In the control 15 % HCl solution, the Nyquist plot (Fig. 4b inset) represents a depressed semicircle with solution (Rs) and charge transfer (Rct) resistances of 1.18 and 30.27 Ωcm2, respectively. In a blank solution, the Nyquist plot is characterized by a single capacitive loop, a trait ascribed to characteristics of a solid electrode surface showing a charge transfer controlled mechanism in a corrosive medium [12,33]. The diameter of the depressed semicircles increased for 1, 5, 10, 20, 50, and 100 ppm of inhibitor 3 with that of blank 15 % HCl. This indicates the adsorption of inhibitor 3 on the metal surface by removing the corrosive species, including water molecules. However, the semicircle corresponding to 100 ppm of inhibitor 3 turned out to be smaller than that of 50 ppm. This can be attributed to introducing a 50 ppm inhibitor solution to the corrosive medium that thoroughly covers the mild steel surface. Increasing the inhibitor concentration further doesn't increase adsorption and can cause the desorption of inhibitor molecules that have already been adsorbed [34,35]. Fig. 4c depicts the Bode magnitude and phase angle plots that further confirm the concentration dependency of inhibitor 3, as already evidenced by Nyquist plots [36,37]. In Fig. 4c, the logarithm of modulus impedance (log /Z/) increases proportionately with increasing inhibitor concentration, reaching a maximum value at an inhibitor concentration of 50 ppm.

In Fig. 4c, the phase angle plots responsible for different concentrations of inhibitor 3 are characterized by broad deflection points with respect to that of blank in the high-frequency region. This can be explained by the fact that the electrochemical fitting of neither the Nyquist plots nor the Bode magnitude plots showed the presence of more than one capacitive loop. The adsorbing inhibitor molecules shield the metal surface against HCl attack and might influence the occurrence of a second loop that Bode phase angle graphs show. When inhibitor 3 is not present, the capacitive loop can be explained by a single, one-time constant that represents a single relaxation process. However, the capacitive loops with inhibitor 3, indicating at least two time constants, imply that multiple relaxation processes occur at the surface [38,39]. The phase angle readings were found to be all below 90° in both the presence and absence of inhibitor 3 at various doses. During the relaxation process, a smaller deflection angle (<90°) can be linked to the surface roughness and inhomogeneity of dielectric materials. However, it is clear that the values of phase angle increase with increasing inhibitor concentrations, which signifies more inhibitive performance due to inhibitor adsorption [40,41]. Fig. 5a and b, respectively, show the equivalent circuits used to fit the EIS plots in the absence and presence of inhibitor 3. Equivalent circuits with one (Fig. 5a) and two (Fig. 5b) time constants were adopted to fit EIS plots corresponding to control 15 % HCl and inhibited solutions, respectively. Because of a rough and porous surface that deviates from the optimum behavior of a capacitor, Fig. 5a and b demonstrate the addition of a constant phase element (CPE) in place of a capacitor. The capacitive constants of the EDL (Ydl) and the protective film (Yfm) generated on the mild steel surface as a result of the adsorption of 3 are incorporated into the expression for the CPE impedance function (Eq. (21)). The exponential value n (ndl and nfm for the EDL and protective film, respectively) that determines the electrical behavior is also included in Eq. (21). The EDL can be considered an ideal capacitor if the electrical behavior caused by surface inhomogeneity causes the n value to equate to 1 [42].

ZCPE=Yo−1(jω)−n (21)

Where, Yo represents the capacitive constant, ω is the radial frequency, and j is an imaginary number used to resolve impedance and reactance from pure resistance.

Fig. 5.

Fig. 5

Equivalent circuits for mild steel corrosion in 15 % HCl were utilized to fit the EIS data obtained in the absence (a) and presence (b) of inhibitor 3.

The relevant impedance parameters are generated by fitting the impedance data in the absence and presence of inhibitor 3 using the circuits depicted in Fig. 5a and b are enumerated in Table 3. The chi-squared (χ2) values were found to be < 0.001, indicating that the impedance plots were fitted very well. Almost all of the measured values of ndl and nfm varies in the range of 0.5–1, indicating the presence of a non-ideal capacitor in a charge transfer corrosion process [43,44]. Cdl values were calculated using Eq. (22) and were found to decrease with increasing concentrations. While the Cdl value for the uninhibited solution was found to be 80.69 μF/cm2; it decreased to 59.58, 42.62, 18.37, 8.29, 3.51, and 5.15 μF/cm2 for 1, 5, 10, 20, 50, and 100 ppm solutions, respectively, of inhibitor 3. As more inhibitors adsorb on the metal surface and the thickness of the double layer increases, the Cdl values decrease accordingly (Eq. (23)).

Cdl=Ydl1ndl(1Rs+1Rct)(ndl−1)ndl (22)
Cdl=εoεdA (23)

Where, Cdl, Rs, Rct, and ndl represent the double-layer capacitance, solution resistance, charge-transfer resistance, and surface inhomogeneity, respectively, and A, d, εo, and ε denote the exposed metal surface area, EDL thickness, permittivity of air, and relative permittivity, respectively.

Table 3.

The parameters of electrochemical impedance were acquired by fitting the Nyquist and Bode plots that were recorded for mild steel corrosion at 30 °C in 15 % HCl with and without inhibitor 3.

Conc. (ppm) Rs (Ωcm2) CPEfm
CPEdl
RT (Ωcm2) ηEIS (%) χ2× 10−3
Yfm (μScm2) nfm Rfm (Ωcm2) Ydl (μScm2) ndl Rct (Ωcm2) Cdl (μF/cm2)
Blank 1.18 – – – 327.1 0.85 30.27 80.69 30.27 – 0.75
1 1.29 3438 0.73 0.70 280.5 0.89 31.02 59.58 31.72 4.60 0.35
5 1.38 20660 1.00 0.28 278 0.81 59.75 42.62 60.03 49.6 0.64
10 1.30 332600 1.00 10.16 212.8 0.77 121.8 18.37 131.96 77.1 1.58
20 1.56 1294 0.64 7.72 117.9 0.76 286.8 8.29 294.52 89.7 0.47
50 2.09 74.36 0.78 388.80 110.8 0.71 180.1 3.51 568.90 94.7 0.32
100 2.08 30.89 0.80 390.10 120.3 0.62 110.57 5.15 500.67 94.0 0.48

The Rct values were also found to be increasing in relation to blank with increasing inhibitor concentrations. This indicates that the transfer/movement of Fe2+/Fe3+ and other corrosive species across the EDL becomes increasingly difficult with additional film formation [45,46]. The adsorption of inhibitor 3 on the metal surface is strongly supported by the rise in Rct values and decrease in Cdl values. This also testifies to the dependency of the IE on the concentration of the inhibitor until a certain dosage. As such, the IEs from the EIS technique were found to be 4.6, 49.6, 77.1, 89.7, 94.7, and 94.0 % for 1, 5, 10, 20, 50, and 100 ppm, respectively, of inhibitor adsorption.

3.3.3. Polarization measurements

Fig. 6a and b, respectively, show polarization measurements obtained at 303 K using linear polarization resistance (LPR) and potentiodynamic polarization (PDP) techniques. It showed that the extent of current density increased after the cathodic and anodic areas experienced a rise in the applied potential. Fig. 6a illustrates that an activation-controlled mechanism is in play for the metal corrosion in the studied acidizing solution. A number of significant electrochemical parameters were obtained by fitting the Tafel curves' cathodic and anodic lines, listed in Table 4. These electrochemical characteristics include the corrosion potential (Ecorr), the corrosion current density (icorr), the anodic (βa) and cathodic (βc) Tafel slopes, etc. The Ecorr of the blank solution was found to be – 466 mV vs. SCE, which is still very close to that of – 510 mV for the blank recorded during OCP curves analysis. Ecorr values recorded for different inhibited solutions in the presence of inhibitor 3 were also close to those found during OCP curves recording. This demonstrates that during the PDP measurements, there was minimal potential drift. Furthermore, none of the inhibited solutions' Ecorr values differed from the blank by more than 85 mV. As previously found during the investigation of OCP curves, this suggests that inhibitor 3 is a mixed-type inhibitor that affects both half-cell reactions. This means that the adsorption of inhibitor 3 reduces the metal's anodic dissolution rates and the cathodic evolution of molecular hydrogen to more or less the same extent. Additionally, the reduction of the corrosion rate without the Ecorr values being significantly altered implies the pickling-type behavior of inhibitor 3 [[47], [48], [49], [50]]. The βa and βc values for the blank solution changed from 99.9 to 127 mV dec−1 to 97.7 and 128 mV dec−1, respectively, for 1 ppm of inhibitor 3. The deviations were significantly more noticeable when inhibitor 3 concentration rose. This again reveals that the adsorption of inhibitor 3 on the metal surface affects both the cathodic and anodic processes. However, when the polarization potential varies during PDP measurements, the disproportionate fluctuations in βa and βc values can be explained by the various degrees of mild steel surface roughness. When inhibitor 3 is not present, the icorr value is 803 μA cm−2. In presence of 1, 5, 10, 20, 50, and 100 ppm of 3, icorr values reduced to 766, 331, 170, 120, 64.9, and 51.9 μA cm−2, respectively. This demonstrates that adding an inhibitor to a corrosive 15 % HCl reduces the corrosion rate significantly, and this effect is the most prominent for 50 ppm of inhibitor 3. Therefore, the IE values, calculated following Eq. (5), corresponding to different concentrations of inhibitor 3 increase as the icorr values decrease in the series.

Fig. 6.

Fig. 6

Tafel curves (a) and linear polarization lines (b) following polarization measurements conducted in blank and inhibited solutions.

Table 4.

PDP and LPR electrochemical parameters following the fitting of polarization curves recorded in both blank and inhibited solutions.

Conc. (ppm)

PDP



LPR
Ecorr (mV) βa (mV dec−1) ‒βc (mV dec−1) Icorr (μA.cm−2) ηPDP (%) Rp (Ωcm2) ηLPR (%)
Blank −466 99.9 127 803 – 28.5 –
1 −468 97.7 128 766 4.6 29.9 4.7
5 −462 112 125 331 58.8 63.6 55.2
10 −468 113 120 170 78.8 138 79.3
20 −475 139 146 120 85.1 311 90.8
50 −479 164 157 64.9 91.9 600 95.2
100 −476 128 140 51.9 93.5 575 95.0

Fig. 6b shows that when the concentration of 3 in the solution rises, the LPR lines progressively tilt toward zero current. Therefore, with increasing concentration of 3, mild steel surface experiences better protection. The IE values from LPR measurements were calculated following Eq. (6) after estimating the LPR line slopes as Rp. The values of Rp and ηLPR(%) are enumerated in Table 4. In the absence of inhibitor 3, the Rp was recorded to be 28.5 Ωcm2. The Rp values kept increasing with increasing inhibitor concentration. From 28.5 Ωcm2 for blank, the Rp values increased to 29.9, 63.6, 138, 311, 600, and 575 Ωcm2 in the presence of 1, 5, 10, 20, 50, and 100 ppm of inhibitor 3. Consequently, the IE values kept rising as well. In presence of 1, 5, 10, 20, 50, and 100 ppm of 3, ηLPR(%) values were calculated as 4.70, 55.2, 79.3, 90.8, 95.2, and 95.0 %, respectively. PDP and LPR procedures produced IE values consistent with WL and EIS techniques.

3.4. Surface studies

3.4.1. SEM-EDX

After completely submerging in the examined electrolyte at 303 K with and without 50 ppm inhibitor 3, the surface appearance and constituent compositions of the metal coupons were examined, as shown in Fig. 7. The surface appearance and elemental composition of a polished, clean, mild steel surface are shown in Fig. 7a. The surface looks nice and smooth without any sign of roughness or cracks. EDX analysis showed the presence of Fe (98.9 %) and other atoms relevant to mild steel. Fig. 7b shows the surface morphology and EDX spectrum of the mild steel surface treated in 15 % HCl without any inhibitor. The surface looks very uneven and rough, with multiple sights showing the attack of Cl− ions. In the absence of any inhibitor, the mild steel surface wasn't offered any protection and was corroded severely. This caused a slight reduction in the elemental composition of Fe (98.5 %) and showed the presence of an additional Cl peak (0.2 %). Fig. 7c depicts the surface morphology and EDX spectra of a mild steel surface treated in 15 % HCl with 50 ppm inhibitor 3. Compared to the surface shown in Fig. 7b, the inhibitor-protected surface in Fig. 7c is much smoother, with one or two sights of aggressiveness from the Cl− ions. The EDX spectrum shows a peak for the presence of C (11.8 %), which originated from the adsorption of inhibitor 3. Interestingly, the wt.% of the Cl peak increased from 0.2 % for the corroded surface to 0.4 % for the inhibited surface owing to the presence of Cl− counters ions present in the inhibitor molecules. Therefore, the existence of a reasonably extended hydrophobic alkyl chain length, a positively charged quaternary ammonium moiety, π-electrons, and unquenched electrons on nitrogen in the diallylamine moiety have all helped inhibitor 3 to act as an excellent corrosion inhibitor.

Fig. 7.

Fig. 7

SEM micrographs (left) and EDX spectra (right) of clean (a), corroded (b), and inhibitor 3-protected (c) metal surfaces.

3.4.2. XPS

XPS survey spectrum and the deconvoluted spectra for Fe2p, N1s, C1s, O1s, and Cl2p, achieved following XPS experiments and software fittings, are shown in Fig. 8. In the survey spectrum (Fig. 8a), Fe2p, O1s, C1s, and Cl2p are very clearly visible along with some other peaks relevant to mild steel. However, the peak for N1s is barely noticeable because nitrogen's contribution to the overall composition of inhibitor 3 is minimal, and only a small amount of inhibitor 3 is present in the corrosive medium. The deconvoluted Fe2p spectrum (Fig. 8b) shows two spin orbitals (2p1/2 and 2p3/2) comprising both Fe2+ and Fe3+ without satellite peaks [51,52]. The percentage composition of Fe (II) and Fe(II) species that are anticipated to form various chlorides, oxides, carbides, and hydroxides [53] are 75.69 and 24.31 %, respectively (Table 5). In Fig. 8c, the presence of two peaks at 402.58 (74.4 %) and 391.48 eV (25.6 %) can be correlated with NH4+ salt and C–N, respectively [[53], [54], [55]]. These two peaks' existence in the deconvoluted spectra of N1s indicates that the inhibitor adheres to the metal surface. In C1s deconvoluted spectrum (Fig. 8d), the presence of a high atomic wt% (70.75 %) peak at 284.88 eV and relatively lower atomic wt% (29.25) eV at 286.68 eV are ascribed to C–C and C–N, respectively [56,57], owing to mild steel surface accommodating the long alkyl hydrophobic chain and nitrogen atoms from inhibitor 3. The presence of a high atomic wt% (83.08 %) peak at 198.88 eV in the Cl2p deconvoluted spectrum (Fig. 8e) can be traced to the presence of FeCl2 and FeCl3 species (Fe–Cl) on the metal surface [25]. An additional peak at more than 200 eV from organic chloride (C–Cl) arises from the interaction between inhibitor 3 and Cl− ions. The deconvoluted O1s spectrum (Fig. 8f) shows a very dominant peak at 532.18 eV and another relatively smaller peak at 530.8 eV owing to O–C–Cl and O–C, respectively [58,59]. These peaks confirm the interactions among oxygen, inhibitor 3, and the Cl− ions present in the corrosive environment. Overall, the detailed analyses based on the interpretation of the presented deconvoluted spectra can be used to establish efficient adsorption of inhibitor 3 on the metal surface.

Fig. 8.

Fig. 8

XPS survey (a) and deconvoluted XPS spectra of Fe2p (b), N1s (c), C1s (d), Cl2p (e), and O1s (f) for mild steel immersed in 15 % HCl in the presence of 50 ppm inhibitor 3 at 30 °C.

Table 5.

Different XPS binding energy (BE) peaks and their relative amounts (%) are assigned to several species.

Element Peak BE (eV) Chemical state Atomic %
Fe2p
710.48 Fe2+ (2p3/2) 57.11
715.98 Fe3+ (2p1/2) 14.58
723.98 Fe2+ (2p3/2) 18.58
729.68
Fe3+ (2p1/2)
9.73
C1s
284.88 C–C 70.75
286.68
C–N
29.25
N1s
402.58 NH4+ salt 74.4
391.48
C–N
25.6
Cl2p
198.88 Fe–Cl 83.08
200.78
C–Cl
16.92
O1s 532.18 O–C–Cl 74.64
530.08 O–C 25.36

3.4.3. Contact angle measurements

The recorded water contact angle values (θH2O) of the polished, corroded, and inhibited mild steel surfaces are shown in Fig. 9. It has been reported that a surface can be susceptible to wetting if its θH2O is lesser than 90° and water-repellent if θH2O is greater than 90° [60]. The polished surface (Fig. 9a) shows a θH2O value of 89.1° indicates that a bare, unexposed surface is considerably hydrophobic. However, when the same surface was exposed to corrosive 15 % HCl at 30 °C, the θH2O value reduced to a very low 20.4° (Fig. 9b). After severe corrosion in 15 % HCl, the surface's hydrophobic nature degrades, and wettability increases. Fig. 9c shows the surface and θH2O value for a mild steel surface treated in 50 ppm of inhibitor 3. The θH2O value for the inhibited surface increased to 98.7° from 20.4° for the corroded one. This demonstrates the inhibitor's efficacy in creating a hydrophobic barrier on the mild steel surface. This hydrophobic barrier limits the contact of water molecules and other aggressive corrosive ions with the metal surface.

Fig. 9.

Fig. 9

The surfaces of polished (a), corroded (b), and inhibited (c) mild steel coupons show water contact angle values.

3.5. Density functional theory calculations

The DFT-optimized structure and the frontier orbitals of inhibitor 3 are depicted in Fig. 10. Different theoretical parameters derived from the calculations are outlined in Table 6. It has been observed from Fig. 10 that the HOMO and LUMO regions are consolidated over the chloride counter ions and the quaternary ammonium and aromatic ring moieties, respectively. The inhibitor's HOMO and LUMO orbitals interact with the metal surface via electron donation and acceptance, respectively [61]. Therefore, it's evident that the chloride counter ions, the quaternary ammonium moiety, and the aromatic ring are crucial to the success of the inhibitor in mitigating mild steel corrosion in 15 % HCl. With an increase in EHOMO, therefore, decrease in ΔE, the ability of the inhibitor molecules to form bonds with the metal surface has been reported to increase [62]. While a low value of ΔE is desired for better efficiency, inhibitor 3 having a HOMO-LUMO energy gap of 7.784 eV indicates a relatively easier movement of electrons from the inhibitor to the surface. The ionization energy (IE) parameter is directly related to EHOMO. The low lying IE value of only 5.865 eV indicates that it’s relatively easier for inhibitor 3 to be ionized and donate electrons to the metal surface. On the other hand, a very low value of – 1.973 eV for electronegativity (χ) indicates that the inhibitor is more prone to donate electrons to the metal surface to promote surface coverage, as the first ionization energy of iron is ~ 8 eV. The calculation of the hardness (η) and softness (σ) values are very important, as they reveal the efficacy of anticorrosion compounds. Usually, low hardness (η) and high softness (σ) values are desirable. The electrophilicity (ω) parameter also plays a vital role in dictating how efficient a corrosion inhibitor is. This parameter expresses the propensity of inhibitor molecules to receive electrons from the metal surface through retro-donation/backdonation [63]. A relatively high value of 7.578 eV for the electrophilicity parameter suggests that the inhibitor interacts strongly with the metal surface via retro-donation. If the fraction of electrons transferred, ΔN, is less than zero (ΔN < 0), the electrons are moving from the metal surface to the inhibitor. On the other hand, if ΔN > 0, it indicates that the electrons are moving from the inhibitor to the metal surface [64]. The latter (ΔN > 0) is the preferred situation for the interaction of inhibitor 3 with the mild steel surface. The dipole moment (μ) metric indicates a molecule's overall polarity or separation between negative and positive charges. Higher μ values result in stronger adsorption of the inhibitor molecule onto the mild steel surface due to intramolecular interactions [65]. A very high value of 26.37 D has been observed for inhibitor 3, indicating its strong adsorption on the metal surface.

Fig. 10.

Fig. 10

Optimized structure (a), HOMO (b), and LUMO (c) of inhibitor 3.

Table 6.

DFT parameters of inhibitor 3 using B3LYP functional and 6-31G+(d,p) basis set.

EHOMO(eV) ELUMO(eV) ΔE(eV) IE(eV) η(eV) χ(eV) ω(eV) σ(eV) ΔN μ
−5.865 1.919 7.784 5.865 3.892 1.973 7.578 0.257 0.367 26.37

3.6. Mechanism of inhibition

The adsorption isotherm studies discussed earlier showed that the ΔGads° for the adsorption of inhibitor 3 on the mild steel surface was – 40.19 kJ mol−1. This allowed us to confer that the adsorption of inhibitor 3 onto a mild steel surface follows a mixed physisorption-chemisorption mechanism. DFT studies provided a testament to this finding. Following quantum chemical calculations, HOMO and LUMO sights that interact with the metal surface through electron donation and acceptance, respectively, were revealed. It was shown that the HOMO is entirely concentrated on the chloride counter ions while the LUMO is spread over the quaternary ammonium and aromatic moieties. Fig. 11 shows how inhibitor 3 can interact with the metal surface through different functionalities embedded in the molecule. The chloride counter ions in the inhibitor, rich in electrons, can donate electrons to the empty d-orbitals of metal atoms, thereby contributing to the chemisorption nature of the overall mechanism.

Fig. 11.

Fig. 11

A schematic representation of how inhibitor 3 interacts with mild steel surface to provide protection.

On the other hand, the positively charged nitrogen ion in the quaternary ammonium moiety can afford an electrostatic interaction with the pre-adsorbed chloride ions (from 15 % HCl) on the metal surface, contributing to the physisorption nature of the overall mechanism. DFT studies showed that the aromatic ring also plays a role. Since the aromatic ring is part of the LUMO, as per the DFT study, the only way the aromatic ring could interact with the metal surface in this circumstance is through retro-donation. Retro-donation, also known as backdonation, happens when the metal atoms' filled d-orbitals donate electrons to the inhibitor's empty p-orbitals. The DFT-derived calculation of a high electrophilicity value (ω) supports the phenomenon of retro-donation as well. The synergism between donation (pπ–dπ) and retro-donation (dπ–pπ) strengthens the inhibition mechanism. Additionally, inhibitor 3 has a favorably long alkyl chain that acts as a hydrophobe. When inhibitor 3 is adsorbed on the surface, this hydrophobic alkyl chain length assists the metal surface by driving away corrosive water molecules. This was further confirmed by the water contact angle analysis discussed earlier.

3.6.1. Comparative inhibition performance of inhibitor 3

Some recently reported monocationic and dicationic surfactant corrosion inhibitors of steels in different HCl acid media are enumerated in Table 7. The IEs obtained from these inhibitors are all very inspiring. All reported inhibitors were tested to protect the corresponding steel structures with very high efficiency. One ubiquitous characteristic feature of these inhibitor molecules is that they all possess one/two quaternary ammonium moieties. This indicates the efficacy of quaternary ammonium compounds in arresting the corrosion of steels in acid media, which inspired the current study. A spacer between the two quaternary ammonium moieties can be entirely hydrophobic [[66], [72], [73], [74]] or contain some heteroatoms with lone pairs [[68], [69], [70]] to make coordination bonds with the empty d-orbitals in the metal atoms. What makes our proposed inhibitor (inhibitor 3: the last entry in Table 7) impart such a high IE for a relatively much smaller concentration (0.1 mM, 50 ppm) than other inhibitors here is possibly a good balance between hydrophobicity, hydrophilicity, and structure simplicity. The presence of the positively charged quaternary ammonium moiety to make electrostatic interactions with the metal surface, the availability of an aromatic ring to experience retrodonation from the metal surface, nitrogen with available lone pair for chelation, and long alkyl chain length to repulse the water molecules are behind the success of the inhibitor. Other inhibitors [[68], [69], [70]] with similar features as inhibitor 3, at the expense of more concentration, registered similar IEs.

4. Conclusions

A new quaternary ammonium salt-based corrosion inhibitor 3 with hydrophobic dodecyl group and electron-rich diallylbenzyl amine moiety has been synthesized and characterized. The corrosion inhibitor was tested for suppressing mild steel corrosion in 15 % HCl at 30 °C utilizing gravimetric and electrochemical corrosion tests. Inhibitor 3 registered a very high IE of ≈95.0 % at just 50 ppm, determined via the LPR technique. Furthermore, the IEs registered using various procedures were in close agreement and found to be 94.2, 94.7, 91.9, and 95.2 %, determined via WL, EIS, PDP, and LPR techniques. Following the effect of temperature (303–333 K) on the IE, inhibitor 3 was found to desorb slowly from the metal surface to register 91.3, 82.8, and 75.0 % IE at 40, 50, and 60 °C. ΔGads° A value of – 40.19 kJ mol−1 was determined via an isotherm study, which revealed that inhibitor 3 adsorbs via a mixed physi-chemisorption mechanism. An increase in the Ea value for blank from 65 kJ mol−1 to 107.4 kJ mol−1 for 50 ppm inhibited solution suggested a significant decrease in metal corrosion. Additionally, a steep increase in ΔSads° value from – 10.3 J mol−1 K−1 for uninhibited (blank) to 106.1 J mol−1 K−1 for inhibited solution indicated the removal of water molecules from the metal surface. DFT studies revealed the HOMO and LUMO sights that interact with the metal surface to confirm the mixed physi-chemisorption mode of adsorption. PDP studies showed that inhibitor 3 retarded the rate of mild steel corrosion by inhibiting both half-cell reactions, which was confirmed by offering discussions on the change of Ecorr and Tafel slope values. A decrease in icorr and Rp values were observed through polarization studies that confirmed the efficacy of inhibitor 3. EIS studies showed that Rct values increased and Cdl values decreased with increasing inhibitor concentration. In-depth SEM-EDX and XPS experiments provided strong evidence for inhibitor 3 adsorption on mild steel surfaces. The water contact angle value for inhibited mild steel surface increased to 98.7° from only 20.4° for uninhibited surface, indicating inhibitor 3's excellent ability to impart hydrophobicity to mild steel surface in solution. Overall, inhibitor 3 successfully inhibited the corrosion of mild steel in 15 % HCl at 30 °C for just a small dose of 0.1 mM (50 ppm). At a very high temperature of 60 °C, the inhibitor still showed 75.0 % IE, which is very promising. In the future, we plan to increase the IE of the inhibitor for high-temperature acid corrosion applications by modifying the hydrophobic chain length and incorporating electro-donating groups in the benzene ring. This could make the modified version of inhibitor 3 considerably less prone to desorption and will be tremendously applicable for very high temperatures.

Data availability

The data is available upon request.

CRediT authorship contribution statement

Lipiar K.M.O. Goni: Writing – original draft, Visualization, Methodology, Investigation, Formal analysis. Shaikh A. Ali: Writing – review & editing, Resources, Project administration, Methodology, Conceptualization. Hasan A. Al-Muallem: Writing – review & editing, Resources. Mohammad A. Jafar Mazumder: Writing – review & editing, Supervision, Resources, Methodology, Funding acquisition, Conceptualization.

Declaration of competing interest

The authors declare no conflict of interest.

Acknowledgements

The authors sincerely acknowledge the research facilities provided by King Fahd University of Petroleum and Minerals (KFUPM) in Saudi Arabia.

Footnotes

Appendix A

Supplementary data to this article can be found online at https://doi.org/10.1016/j.heliyon.2024.e38425.

Appendix A. Supplementary data

The following is/are the supplementary data to this article.

Multimedia component 1
mmc1.docx (146.3KB, docx)

References

  • 1.Mccafferty E. first ed. Springer-Verlag; New York: 2010. Introduction to Corrosion Science. [Google Scholar]
  • 2.Javaherdashti R. How corrosion affects industry and life. Anti-Corros Methods Mater. 2000;47:30–34. doi: 10.1108/00035590010310003. [DOI] [Google Scholar]
  • 3.Emmanuel J.K. Corrosion protection of mild steel in corrosive media, a shift from synthetic to natural corrosion inhibitors: a review. Bull. Natl. Res. Cent. 2024;48:26. doi: 10.1186/s42269-024-01181-7. [DOI] [Google Scholar]
  • 4.Wang J., Wang Y., Yang Z., Guo L., Yang J., Yang Q., Wu J. Synthesis of a novel fused heterocyclic quaternary ammonium salt and its performance in ultra-low dosage as acidizing corrosion inhibitor. J. Mol. Struct. 2024;1303 doi: 10.1016/j.molstruc.2024.137571. [DOI] [Google Scholar]
  • 5.Koch G., Varney J., Thompson N., Moghissi O., Gould M., Payer J. International measures of prevention, application, and economics of corrosion technologies study. 2024. http://impact.nace.org/
  • 6.Yaagoob I.Y., Goni L.K.M.O., Mazumder M.A.J., Ali S.A., Quraishi M.A., Verma C. Synthesis of polymeric surfactant containing bis-cationic motifs as a highly efficient acid corrosion inhibitor for C1018 carbon steel. New J. Chem. 2023;47:3445–3461. doi: 10.1039/d2nj05978a. [DOI] [Google Scholar]
  • 7.Verma C., Ebenso E.E., Quraishi M.A., Hussain C.M. Recent developments in sustainable corrosion inhibitors: design, performance and industrial scale applications. Mater Adv. 2021;2:3806–3850. doi: 10.1039/d0ma00681e. [DOI] [Google Scholar]
  • 8.Alharbi B., Aljeaban N., Goni L.K.M.O., Jafar Mazumder M.A., Chen T., Buhaezah W., Ali S.A. Synthesis and investigation of two new compounds (2-(methoxymethyl)−1- phenyl-2-propen-1-one and 2-(methoxymethyl)−1-(4-methoxyphenyl) - 2-Propen-1-one) as corrosion inhibitors for mild steel in acidic solutions at elevated temperature. Int. J. Electrochem. Sci. 2024;19 doi: 10.1016/j.ijoes.2024.100508. [DOI] [Google Scholar]
  • 9.Al-Rawajfeh A.E., Al-Shamaileh E.M. Inhibition of corrosion in steel water pipes by ammonium pyrrolidine dithiocarbamate (APDTC) Desalination. 2007;206:169–178. doi: 10.1016/j.desal.2006.02.065. [DOI] [Google Scholar]
  • 10.Nahlé A.H., Harvey T.J., Walsh F.C. Quaternary aryl phosphonium salts as corrosion inhibitors for iron in HCl. J. Alloys Compd. 2018;765:812–825. doi: 10.1016/j.jallcom.2018.06.241. [DOI] [Google Scholar]
  • 11.Haque J., Jafar Mazumder M.A., Quraishi M.A., Ali S.A., Aljeaban N.A. Pyrrolidine-based quaternary ammonium salts containing propargyl and hydrophobic C-12 and C-16 alkyl chains as corrosion inhibitors in aqueous acidic media. J. Mol. Liq. 2020;320 doi: 10.1016/j.molliq.2020.114473. [DOI] [Google Scholar]
  • 12.Odewunmi N.A., Mazumder M.A.J., Ali S.A., Alharbi B.G. Hydroquinone decorated with alkyne, quaternary ammonium, and hydrophobic motifs to mitigate corrosion of X-60 mild steel in 15 wt.% HCl. Chem. Asian J. 2021;16:801–821. doi: 10.1002/asia.202100085. [DOI] [PubMed] [Google Scholar]
  • 13.Chauhan D.S., Quraishi M.A., Jafar Mazumder M.A., Ali S.A., Aljeaban N.A., Alharbi B.G. Design and synthesis of a novel corrosion inhibitor embedded with quaternary ammonium, amide and amine motifs for protection of carbon steel in 1 M HCl. J. Mol. Liq. 2020;317 doi: 10.1016/j.molliq.2020.113917. [DOI] [Google Scholar]
  • 14.Jalab R., Saad M.A., Sliem M.H., Abdullah A.M., Hussein I.A. An eco-friendly quaternary ammonium salt as a corrosion inhibitor for carbon steel in 5 M HCl solution: theoretical and experimental investigation. Molecules. 2022;27:6414. doi: 10.3390/molecules27196414. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 15.El-Tabei A.S., El-Azabawy O.E., El Basiony N.M., Hegazy M.A. Newly synthesized quaternary ammonium bis-cationic surfactant utilized for mitigation of carbon steel acidic corrosion; theoretical and experimental investigations. J. Mol. Struct. 2022;1262 doi: 10.1016/j.molstruc.2022.133063. [DOI] [Google Scholar]
  • 16.Zheng T., Liu J., Wang M., Liu Q., Wang J., Chong Y., Jia G. Synergistic corrosion inhibition effects of quaternary ammonium salt cationic surfactants and thiourea on Q235 steel in sulfuric acid: experimental and theoretical research. Corros Sci. 2022;199 doi: 10.1016/j.corsci.2022.110199. [DOI] [Google Scholar]
  • 17.Saad I.R., Abdel-Gaber A.M., Younes G.O., Nsouli B. Thiourea and N-methylthiourea as corrosion inhibitors for steel in phosphoric acid. J. Fail. Anal. Prev. 2018;18:1293–1299. doi: 10.1007/s11668-018-0522-5. [DOI] [Google Scholar]
  • 18.El Sayed M.Y., Abdel-Gaber A.M., Rahal H.T. Safranin—a potential corrosion inhibitor for mild steel in acidic media: a combined experimental and theoretical approach. J. Fail. Anal. Prev. 2019;19:1174–1180. doi: 10.1007/s11668-019-00719-6. [DOI] [Google Scholar]
  • 19.Yaagoob I.Y., Goni L.K.M.O., Verma C., Mazumder M.A.J., Ali S.A. N-(4-Chloromethylbenzyl)-N, N-dimethyldodecan-1-aminium chloride: a quaternary ammonium surfactant as corrosion inhibitor. ChemistrySelect. 2023;8:483–496. doi: 10.1002/slct.202301913. [DOI] [Google Scholar]
  • 20.Shariatinia Z., Ahmadi-Ashtiani A. Corrosion inhibition efficiency of some phosphoramide derivatives: DFT computations and MD simulations. J. Mol. Liq. 2019;292 doi: 10.1016/j.molliq.2019.111409. [DOI] [Google Scholar]
  • 21.Sebhaoui J., El Bakri Y., El Aoufir Y., Anouar E.H., Guenbour A., Nasser A.A., Mokhtar Essassi E. Synthesis, NMR characterization, DFT and anticorrosion on carbon steel in 1M HCl of two novel 1,5-benzodiazepines. J. Mol. Struct. 2019;1182:123–130. doi: 10.1016/j.molstruc.2019.01.037. [DOI] [Google Scholar]
  • 22.Vaszilcsin N., Kellenberger A., Dan M.L., Duca D.A., Ordodi V.L. Efficiency of expired drugs used as corrosion inhibitors: a review. Materials. 2023;16:5555. doi: 10.3390/ma16165555. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 23.Han T., Guo J., Zhao Q., Wu Y., Zhang Y. Enhanced corrosion inhibition of carbon steel by pyridyl gemini surfactants with different alkyl chains. Mater. Chem. Phys. 2020;240 doi: 10.1016/j.matchemphys.2019.122156. [DOI] [Google Scholar]
  • 24.Umoren S.A., Solomon M.M., Ali S.A., Dafalla H.D.M. Synthesis, characterization, and utilization of a diallylmethylamine-based cyclopolymer for corrosion mitigation in simulated acidizing environment. Mater Sci Eng C. 2019;100:897–914. doi: 10.1016/j.msec.2019.03.057. [DOI] [PubMed] [Google Scholar]
  • 25.Odewunmi N.A., Mazumder M.A.J., Ali S.A. Evaluation of 1-hexadecylbenzimidazole as a corrosion inhibitor on low carbon steel 15 % HCl solution interface. ChemistrySelect. 2021;6:3199–3217. doi: 10.1002/slct.202100326. [DOI] [Google Scholar]
  • 26.Lai C., Xie B., Zou L., Zheng X., Ma X., Zhu S. Adsorption and corrosion inhibition of mild steel in hydrochloric acid solution by S-allyl-O,O′-dialkyldithiophosphates. Results Phys. 2017;7:3434–3443. doi: 10.1016/j.rinp.2017.09.012. [DOI] [Google Scholar]
  • 27.Akinbulumo O.A., Odejobi O.J., Odekanle E.L. Thermodynamics and adsorption study of the corrosion inhibition of mild steel by Euphorbia heterophylla L. extract in 1.5 M HCl. Results Mater. 2020;5 doi: 10.1016/j.rinma.2020.100074. [DOI] [Google Scholar]
  • 28.Afia L., Benali O., Salghi R., Ebenso E.E., Jodeh S., Zougagh M., Hammouti B. Steel corrosion inhibition by acid garlic essential oil as a green corrosion inhibitor and sorption behavior. Int. J. Electrochem. Sci. 2014;9:8392–8406. doi: 10.1016/S1452-3981(23)11055-8. [DOI] [Google Scholar]
  • 29.Mohsenifar F., Jafari H., Sayin K. Investigation of thermodynamic parameters for steel corrosion in acidic solution in the presence of N,N′-bis(phloroacetophenone)-1,2 propanediamine. J Bio Tribocorros. 2016;2:1. doi: 10.1007/s40735-015-0031-y. [DOI] [Google Scholar]
  • 30.Solomon M.M., Umoren S.A., Quraishi M.A., Tripathy D.B., Abai E.J. Effect of alkyl chain length, flow, and temperature on the corrosion inhibition of carbon steel in a simulated acidizing environment by an imidazoline-based inhibitor. J. Pet. Sci. Eng. 2020;187 doi: 10.1016/j.petrol.2019.106801. [DOI] [Google Scholar]
  • 31.Umoren S., Obot I.B., Gasem Z., Odewunmi N.A. Experimental and theoretical studies of red apple fruit extract as green corrosion inhibitor for mild steel in HCl solution. J. Dispersion Sci. Technol. 2015;36:789–802. doi: 10.1080/01932691.2014.922887. [DOI] [Google Scholar]
  • 32.Abd El-Lateef H.M. Corrosion inhibition characteristics of a novel salycilidene isatin hydrazine sodium sulfonate on carbon steel in HCl and a synergistic nickel ions additive: a combined experimental and theoretical perspective. Appl. Surf. Sci. 2020;501 doi: 10.1016/j.apsusc.2019.144237. [DOI] [Google Scholar]
  • 33.Han T., Guo J., Zhao Q., Wu Y., Zhang Y. Enhanced corrosion inhibition of carbon steel by pyridyl gemini surfactants with different alkyl chains. Mater. Chem. Phys. 2020;240 doi: 10.1016/j.matchemphys.2019.122156. [DOI] [Google Scholar]
  • 34.Alhaffar M.T., Umoren S.A., Obot I.B., Ali S.A. Isoxazolidine derivatives as corrosion inhibitors for low carbon steel in HCl solution: experimental, theoretical and effect of KI studies. RSC Adv. 2018;8:1764–1777. doi: 10.1039/c7ra11549k. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 35.Odewunmi N.A., Umoren S.A., Gasem Z.M. Utilization of watermelon rind extract as a green corrosion inhibitor for mild steel in acidic media. J. Ind. Eng. Chem. 2015;21:239–247. doi: 10.1016/j.jiec.2014.02.030. [DOI] [Google Scholar]
  • 36.Moselhy M.A., Zaki E.G., El-Maksoud S.A.E.H.A., Migahed M.A. Surface activity and electrochemical behavior of some thiazine cationic surfactants and their efficiency as corrosion inhibitors for carbon steel in a sour environment. ACS Omega. 2021;6:19559–19568. doi: 10.1021/acsomega.1c02005. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 37.Kharbouch O., Dahmani K., Errahmany N., Belkheiri A., Galai M., El Hajri F., Alobaid A.A., Warad I., Boukhris S., Ebn Touhami M., Nassali H. Enhancing corrosion resistance of mild steel in 1M HCl: investigation of new benzoxazepine derivatives through synthesis, electrochemical analysis, surface analysis, XPS, DFT, and molecular dynamics simulation. ChemistrySelect. 2024;9 doi: 10.1002/slct.202303045. [DOI] [Google Scholar]
  • 38.Khanra A., Gayen R.N. Distribution of relaxation time in solution-processed polycrystalline CZTS thin films: study of impedance spectroscopy. Ceram. Int. 2018;44:14095–14100. doi: 10.1016/j.ceramint.2018.05.007. [DOI] [Google Scholar]
  • 39.Arrousse N., Fernine Y., Al-Zaqri N., Boshaala A., Ech-Chihbi E., Salim R., El Hajjaji F., Alami A., Touhami M.E., Taleb M. Thiophene derivatives as corrosion inhibitors for 2024-T3 aluminum alloy in hydrochloric acid medium. RSC Adv. 2022;12:10321–10335. doi: 10.1039/d2ra00185c. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 40.Xavier Stango S.A., Vijayalakshmi U. Studies on corrosion inhibitory effect and adsorption behavior of waste materials on mild steel in acidic medium. J Asian Ceramic Soc. 2018;6:20–29. doi: 10.1080/21870764.2018.1439608. [DOI] [Google Scholar]
  • 41.Hosny S., Abdelfatah A., Gaber G.A. Synthesis, characterization, synergistic inhibition, and biological evaluation of novel Schiff base on 304 stainless steel in acid solution. Sci. Rep. 2024;14:470. doi: 10.1038/s41598-023-51044-w. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 42.Shao S., Wu B., Wang P., He P., Qu X.P. Investigation on inhibition of ruthenium corrosion by glycine in alkaline sodium hypochlorite based solution. Appl. Surf. Sci. 2020;506 doi: 10.1016/j.apsusc.2019.144976. [DOI] [Google Scholar]
  • 43.Kalia V., Kumar P., Kumar S., Goyal M., Pahuja P., Jhaa G., Lata S., Dahiya H., Kumar S., Kumari A., Verma C. Synthesis, characterization and corrosion inhibition potential of oxadiazole derivatives for mild steel in 1M HCl: electrochemical and computational studies. J. Mol. Liq. 2022;348 doi: 10.1016/j.molliq.2021.118021. [DOI] [Google Scholar]
  • 44.Kumar S., Kalia V., Goyal M., Jhaa G., Kumar S., Vashisht H., Dahiya H., Quraishi M.A., Verma C. Newly synthesized oxadiazole derivatives as corrosion inhibitors for mild steel in acidic medium: experimental and theoretical approaches. J. Mol. Liq. 2022;357 doi: 10.1016/j.molliq.2022.119077. [DOI] [Google Scholar]
  • 45.Al-Amiery A.A., Mohamad A.B., Kadhum A.A.H., Shaker L.M., Isahak W.N.R.W., Takriff M.S. Experimental and theoretical study on the corrosion inhibition of mild steel by nonanedioic acid derivative in hydrochloric acid solution. Sci. Rep. 2022;12:4705. doi: 10.1038/s41598-022-08146-8. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 46.Abdul Rahiman A.F.S., Sethumanickam S. Corrosion inhibition, adsorption and thermodynamic properties of poly(vinyl alcohol-cysteine) in molar HCl. Arab. J. Chem. 2017;10:S3358–S3366. doi: 10.1016/j.arabjc.2014.01.016. [DOI] [Google Scholar]
  • 47.Lakbaibi Z., Damej M., Molhi A., Benmessaoud M., Tighadouini S., Jaafar A., Benabbouha T., Ansari A., Driouich A., Tabyaoui M. Evaluation of inhibitive corrosion potential of symmetrical hydrazine derivatives containing nitrophenyl moiety in 1M HCl for C38 steel: experimental and theoretical studies. Heliyon. 2022;8 doi: 10.1016/j.heliyon.2022.e09087. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 48.Damej M., Molhi A., Tassaoui K., El Ibrahimi B., Akounach Z., Addi A.A., El hajjaji S., Benmessaoud M. Experimental and theoretical study to understand the adsorption process of p-anisidine and 4-nitroaniline for the dissolution of c38 carbon steel in 1M HCl. ChemistrySelect. 2022;7 doi: 10.1002/slct.202103192. [DOI] [Google Scholar]
  • 49.El Khatib L.W., Rahal H.T., Abdel-Gaber A.M. Synergistic effect between fragaria ananassa and cucurbita pepo l leaf extracts on mild steel corrosion in hydrochloric acid solutions. Prot Chem Phys Met Surf. 2020;56:1096–1106. doi: 10.1134/S2070205120050111. [DOI] [Google Scholar]
  • 50.Al-Moghrabi R.S., Abdel-Gaber A.M., Rahal H.T. A comparative study on the inhibitive effect of Crataegus oxyacantha and Prunus avium plant leaf extracts on the corrosion of mild steel in hydrochloric acid solution. Int J Ind Chem. 2018;9:255–263. doi: 10.1007/s40090-018-0154-3. [DOI] [Google Scholar]
  • 51.Andrzejewski B., Chybczyńska K., Hilczer B., Błaszyk M., Luciński T., Matczak M., Kępiński L. Controlled growth of bismuth ferrite multiferroic flowers. 2014. https://arxiv.org/abs/1402.1336/
  • 52.Wilson D., Langell M.A. XPS analysis of oleylamine/oleic acid capped Fe3O4 nanoparticles as a function of temperature. Appl. Surf. Sci. 2014;303:6–13. doi: 10.1016/J.APSUSC.2014.02.006. [DOI] [Google Scholar]
  • 53.Paul P.K., Yadav M. Investigation on corrosion inhibition and adsorption mechanism of triazine-thiourea derivatives at mild steel/HCl solution interface: electrochemical, XPS, DFT and Monte Carlo simulation approach. J. Electroanal. Chem. 2020;877 doi: 10.1016/J.JELECHEM.2020.114599. [DOI] [Google Scholar]
  • 54.Gu Y., Chen S., Ren J., Jia Y.A., Chen C., Komarneni S., Yang D., Yao X. Electronic structure tuning in Ni3FeN/r-GO aerogel toward bifunctional electrocatalyst for overall water splitting. ACS Nano. 2018;12:245–253. doi: 10.1021/acsnano.7b05971. [DOI] [PubMed] [Google Scholar]
  • 55.Martins N.C.T., Ângelo J., Girão A.V., Trindade T., Andrade L., Mendes A. N-doped carbon quantum dots/TiO2 composite with improved photocatalytic activity. Appl. Catal., B. 2016;193:67–74. doi: 10.1016/j.apcatb.2016.04.016. [DOI] [Google Scholar]
  • 56.Cao J., Wang Y., Chen J., Li X., Walsh F.C., Ouyang J.-H., Jia D., Zhou Y. Three-dimensional graphene oxide/polypyrrole composite electrodes fabricated by one-step electrodeposition for high-performance supercapacitors. J Mater Chem A Mater. 2015;3:14445–14457. doi: 10.1039/C5TA02920A. [DOI] [Google Scholar]
  • 57.Hashim N.Z.N., Anouar E.H., Kassim K., Zaki H.M., Alharthi A.I., Embong Z. XPS and DFT investigations of corrosion inhibition of substituted benzylidene Schiff bases on mild steel in hydrochloric acid. Appl. Surf. Sci. 2019;476:861–877. doi: 10.1016/J.APSUSC.2019.01.149. [DOI] [Google Scholar]
  • 58.Ralkhal S., Shahrabi T., Ramezanzadeh B., Bahlakeh G. A combined electrochemical, molecular dynamics, quantum mechanics and XPS analysis of the mild steel surface protected by a complex film composed of neodymium (III) and benzimidazole. Appl. Surf. Sci. 2019;464:178–194. doi: 10.1016/J.APSUSC.2018.09.064. [DOI] [Google Scholar]
  • 59.Singh P., Srivastava V., Quraishi M.A. Novel quinoline derivatives as green corrosion inhibitors for mild steel in acidic medium: electrochemical, SEM, AFM, and XPS studies. J. Mol. Liq. 2016;216:164–173. doi: 10.1016/J.MOLLIQ.2015.12.086. [DOI] [Google Scholar]
  • 60.Abdelshafi N.S., Farag A.A., Heakal F.E.T., Badran A.S., Abdel-Azim K.M., Manar El Sayed A.R., Ibrahim M.A. In-depth experimental assessment of two new aminocoumarin derivatives as corrosion inhibitors for carbon steel in HCl media combined with AFM, SEM/EDX, contact angle, and DFT/MDs simulations. J. Mol. Struct. 2024;1304 doi: 10.1016/j.molstruc.2024.137638. [DOI] [Google Scholar]
  • 61.Gutiérrez E., Rodríguez J.A., Cruz-Borbolla J., Alvarado-Rodríguez J.G., Thangarasu P. Development of a predictive model for corrosion inhibition of carbon steel by imidazole and benzimidazole derivatives. Corros Sci. 2016;108:23–35. doi: 10.1016/J.CORSCI.2016.02.036. [DOI] [Google Scholar]
  • 62.Esmaeilzadeh Khabazi M., Najafi Chermahini A. DFT study on corrosion inhibition by tetrazole derivatives: investigation of the substitution effect. ACS Omega. 2023;8:9978–9994. doi: 10.1021/acsomega.2c07185. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 63.Lai Z., Wang S., Wang C., Hong Y., Zhou G., Chen Y., He W., Peng Y., Xiao D. A comparison of typical additives for copper electroplating based on theoretical computation. Comput. Mater. Sci. 2018;147:95–102. doi: 10.1016/J.COMMATSCI.2017.11.049. [DOI] [Google Scholar]
  • 64.Bourzi H., Oukhrib R., El Ibrahimi B., Oualid H.A., Abdellaoui Y., Balkard B., Hilali M., El Issami S. Understanding of anti-corrosive behavior of some tetrazole derivatives in acidic medium: adsorption on Cu (111) surface using quantum chemical calculations and Monte Carlo simulations. Surf. Sci. 2020;702 doi: 10.1016/J.SUSC.2020.121692. [DOI] [Google Scholar]
  • 65.Abdulazeez I., Khaled M., Al-Saadi A.A. Impact of electron-withdrawing and electron-donating substituents on the corrosion inhibitive properties of benzimidazole derivatives: a quantum chemical study. J. Mol. Struct. 2019;1196:348–355. doi: 10.1016/J.MOLSTRUC.2019.06.082. [DOI] [Google Scholar]
  • 66.Wang D., Li Y., Chen B., Zhang L. Novel surfactants as green corrosion inhibitors for mild steel in 15% HCl: experimental and theoretical studies. Chem Eng J. 2020;402 doi: 10.1016/j.cej.2020.126219. [DOI] [Google Scholar]
  • 67.Farag A.A., Abdallah H.E., Badr E.A., Mohamed E.A., Ali A.I., El-Etre A.Y. The inhibition performance of morpholinium derivatives on corrosion behavior of carbon steel in the acidized formation water: theoretical, experimental and biocidal evaluations. J. Mol. Liq. 2021;341 doi: 10.1016/j.molliq.2021.117348. [DOI] [Google Scholar]
  • 68.Kaczerewska O., Leiva-Garcia R., Akid R., Brycki B., Kowalczyk I., Pospieszny T. Effectiveness of O-bridged cationic gemini surfactants as corrosion inhibitors for stainless steel in 3 M HCl: experimental and theoretical studies. J. Mol. Liq. 2018;249:1113–1124. doi: 10.1016/j.molliq.2017.11.142. [DOI] [Google Scholar]
  • 69.Pakiet M., Kowalczyk I., Leiva Garcia R., Akid R., Brycki B. Cationic clevelable surfactants as highly efficient corrosion inhibitors of stainless steel AISI 304: electrochemical study. J. Mol. Liq. 2020;315 doi: 10.1016/j.molliq.2020.113675. [DOI] [Google Scholar]
  • 70.Pakiet M., Kowalczyk I.H., Leiva Garcia R., Akid R., Brycki B.E. Influence of different counterions on gemini surfactants with polyamine platform as corrosion inhibitors for stainless steel AISI 304 in 3 M HCl. J. Mol. Liq. 2018;268:824–831. doi: 10.1016/j.molliq.2018.07.120. [DOI] [Google Scholar]
  • 71.Alnajjar A.O., Abd El-Lateef H.M. A novel approach to investigate the synergistic inhibition effect of nickel phosphate nanoparticles with quaternary ammonium surfactant on the Q235-mild steel corrosion: surface morphology, electrochemical-computational modeling outlines. J. Mol. Liq. 2021;337 doi: 10.1016/j.molliq.2021.116125. [DOI] [Google Scholar]
  • 72.Deyab M.A., Mohsen Q. Inhibitory influence of cationic Gemini surfactant on the dissolution rate of N80 carbon steel in 15% HCl solution. Sci. Rep. 2021;11 doi: 10.1038/s41598-021-90031-x. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 73.Mu’azu N.D., Haladu S.A., AlGhamdi J.M., Alqahtani H.A., Manzar M.S., Zubair M., Odewunmi N.A., Aldossary N.E., Saud alareefi H., Alshaer Z.H., Ali S.A., El-Lateef H.M.A. Inhibition of low carbon steel corrosion by a cationic gemini surfactant in 10wt.% H2SO4 and 15wt.% HCl under static condition and hydrodynamic flow. S. Afr. J. Chem. Eng. 2023;43:232–244. doi: 10.1016/j.sajce.2022.10.006. [DOI] [Google Scholar]
  • 74.Zhang X., Zheng Y., Wang X., Yan Y., Wu W. Corrosion inhibition of N80 steel using novel diquaternary ammonium salts in 15% hydrochloric Acid. Ind. Eng. Chem. Res. 2014;53:14199–14207. doi: 10.1021/ie502405a. [DOI] [Google Scholar]

Associated Data

This section collects any data citations, data availability statements, or supplementary materials included in this article.

Supplementary Materials

Multimedia component 1
mmc1.docx (146.3KB, docx)

Data Availability Statement

The data is available upon request.


Articles from Heliyon are provided here courtesy of Elsevier

RESOURCES