Skip to main content
. 2024 Oct 24;10(23):e39723. doi: 10.1016/j.heliyon.2024.e39723

Table 2.

Physicochemical characterization of catalysts loaded with different amounts of indium.

Catalysts Cu content (wt %)a In content (wt %)a SBETb (m2/g) Vporec (cm3/g) Dpored (nm) Cu Particle size (nm)e Cu Particle size (nm)f
Cu/SiO2 20.8 293.5 0.54 7.4 8.6 5.7
Cu-0.25In/SiO2 20.3 0.26 301.7 0.61 8.1 3.3
Cu-0.5In/SiO2 20.2 0.53 303.9 0.64 8.3 3.7
Cu-1In/SiO2 20.4 1.01 306.1 0.65 8.3 2.6
Cu-2In/SiO2 20.1 2.04 266.3 0.51 7.7 12.7 7.1

Note.

[a]

Determined by ICP-OES analysis.

[b]

Specific surface area.

[c]

Pore volume.

[d]

Pore diameter, P/P0 = 0.995.

[e]

Calculated from XRD.

[f]

Obtained through TEM measurement.