Skip to main content
. 2024 Dec 19;14:30558. doi: 10.1038/s41598-024-78842-0

Table 3.

Mechanical properties of the developed Zn-Mg-Mn alloys.

Alloys (wt%) Processing state UTS (MPa) Elongation (%) Reference
Zn-0.8Mn-0.4Mg Extrusion (230 ℃) 359 5 42
Zn-0.8Mn-0.1Mg Extrusion (200 ℃) 355 19 43
Zn-0.8Mn-1Mg 359 8
Zn-0.6Mn-0.05Mg Extrusion (230 ℃) 345 28 33
Zn-0.8Mn-0.05Mg 356 20
Zn-0.2Mg-0.1Mn Extrusion (200 ℃) 266 23 27
Zn-0.2Mg-0.3Mn 300 27
Zn-0.2Mg-0.5Mn 338 30
Zn-0.2Mg-0.8Mn 383 21
Zn-0.2Mg-0.8Mn Extrusion (150 ℃) 372 33 28
Extrusion (200 ℃) 380 21
Extrusion (250 ℃) 360 19
Extrusion (300 ℃) 360 11
Zn-0.6Mg-0.1Mn ECAP (150 ℃) 358 23 44
Zn-0.1Mg-0.02Mn Rolling (25 ℃) 380 16 45
Zn-0.05Mg-0.1Mn Rolling (25 ℃) 274 41 46
Zn-1Mg-0.1Mn Rolling (250 ℃) 299 26 47
Zn-0.8Mg-0.2Mn Extrusion (150 ℃) 414 26 This work