Skip to main content
3D Printing and Additive Manufacturing logoLink to 3D Printing and Additive Manufacturing
. 2024 Oct 22;11(5):1691–1702. doi: 10.1089/3dp.2022.0262

Evaluation of Tensile Strength and Repeatability of 3D Printed Carbon Fiber Materials and Processes

Abigail Batley 1,✉, Richard Glithro 1, Bryce Dyer 1, Philip Sewell 2
PMCID: PMC11683443  PMID: 39741549

Abstract

As additive manufacturing (AM) with composite materials becomes more widely used in industry to create high-strength components, it is vital to have quantified material properties that provide designers and engineers accurate data to decide which materials are suitable for their applications. This study replicates the build processes and tensile tests undertaken by AM material manufacturers to compare tensile strengths achieved with those stated on the manufacturers' data sheets. These are important data to research and analyze as either it will corroborate properties given by the manufacturers and provide confidence in the values provided or it will show that the manufacturer's values cannot always be achieved and that designers and engineers must be more critical about the values manufacturers are providing when using the materials in their own applications. Tensile tests were performed on additively manufactured specimens that had been built using the same parameters that were used during the manufacturers' testing procedures. Digital image correlation was used to accurately measure strain in the test samples, enabling material properties to be determined. Microscopy analysis enabled the visual inspection of the print quality, the identification of defects, and the determination of volume fraction with the samples. The results show inconsistencies between the tensile strength results achieved during this study and the tensile strengths stated by the manufacturers. The results show that two materials exceeded the expected values and one material did not reach the expected value. Analysis of the 3D printed specimens shows that poor fiber–matrix wetting, large voids, and weak interfacial bonding were accountable for the lower-than-expected tensile strength results. While good print quality, low void percentage, proper fiber–matrix wetting, and good control measures were accountable for results that exceeded expectation. These results show that designers and engineers cannot solely rely on material data sheets to establish the mechanical properties of their 3D printed components.

Keywords: additive manufacturing, composite 3D printing, tensile strength, repeatability, carbon fiber


graphic file with name 3dp.2022.0262_figure9.jpg

Introduction

Fused filament fabrication (FFF) printing technology is the most widely used technology across the additive manufacturing (AM) industry. Its popularity is attributed to its large range of application fields, printable materials, printing simplicity, and printing controls.1,2 Currently, the two main types of 3D composite printing are variations of FFF technologies. The two approaches are printing with short reinforcement fibers mixed with a thermoplastic matrix and continuous composite printing. FFF composite printing allows reinforcements to be accurately placed and structures to be optimized per layer, allowing increased design freedom and mechanical performance.3

Continuous strands of carbon fiber can absorb and distribute loads across their entire length; therefore, when placed within a thermoplastic matrix, the part can handle higher loads and absorb larger impacts in predicted orientations.4 Chopped strands of carbon fibers are chopped into small pieces and mixed into a matrix at uncontrollable angles resulting in the fibers absorbing some of the applied stresses on the part, and increasing properties such as strength, stiffness, and dimensional stability across the entire part in multiple orientations.4

Mechanical properties of thermoplastics used are low in comparison to common engineering materials3 such as aluminum and steel, so adding a reinforcement into the material can increase its mechanical properties and broaden its range of applications. The addition of short carbon fibers (∼0.1 mm) mixed with a thermoplastic polymer can increase the strength and stiffness of the printed material by 65%; however, due to the FFF printing technique, the strength increase can be limited, as fiber pullout may occur before fiber breakage.3

Continuous composite printing involves extruding continuous strands of a reinforcement material, such as carbon fiber into the 3D print. Printing with continuous carbon fibers provides significant increases in performance over unreinforced thermoplastics.3,5 The use of continuous composite 3D printing has opened new applications for fabrication and the manufacture of high-strength lightweight components for industry.3 3D printing with continuous carbon fiber can produce components “8x stronger than ABS and 20% stronger than the yield strength of aluminium,” resulting in parts of strength and stiffness of 700 MPa and 50 GPa, respectively.3 A drawback to this type of composite printing is that the continuous fibers cannot be deposited freely through small steering radii and sharp angles, meaning that some geometries are impossible to print using continuous composite printing.3

In conjunction with the material chosen for part production, the mechanical properties of a 3D printed component can be influenced by the print process. Print parameters that have been found to influence the mechanical properties of a component include layer height, wall thickness, orientation, temperature, infill density, and infill pattern.6 Specifically for composite 3D printing, the infill pattern has been found to significantly impact the mechanical properties.7 Naranjo-Lozada et al. reported increased tensile strength when using triangular infill pattern over rectangular infill pattern for composite 3D printing.

Although data sheets are available for a variety of 3D printable composite materials, the mechanical properties of the printed component can deviate from the stock materials due to the specifics of how a structure is formed on the meso-scale during printing.3 To ensure that 3D printed carbon fiber components meet required design specifications in industrial applications, it is necessary to understand their tensile properties.8 While research has been conducted previously into the tensile properties certain materials possess when printed, research into the mechanical properties which a component has achieved compared against the manufacturer-given values for a variety of composite 3D printed materials is sparse. This study aims to compare the tensile strength and other material properties of carbon fiber 3D printed materials against the values provided by the manufacturers to assess their reliability and repeatability. The main goal of the research was to increase knowledge in the field of 3D printing material properties and their accuracy and reliability.

Materials and Methods

Methodology

The methods used during this research aim to replicate the methodology used by the manufacturers when achieving their material properties results. Replicating the methodology and printing parameters used by the manufacturers will reduce variability and increase reliability in the results achieved when compared against the manufacturer's values. It is vital to replicate their methodology for this comparative research as producing parts with different print parameters would provide completely different material properties. For example, building the specimens in a different orientation will affect its mechanical properties, particularly its anisotropy, and printing with different layer/fiber orientations will affect the mechanical properties of the specimen, including strength, stiffness, and ductility.5,6,9 Specifically, the orientation of the fibers relative to the loading direction can have a significant impact on the strength of the specimen.8,9

An in-depth review of the academic literature was conducted alongside the manufacturers' build processes to ensure that print parameters that would influence the results had been accounted for. This review of the academic literature resulted in the following print parameters being analyzed and matched to the manufacturers' build processes: fill density, layer/fiber orientation, slicing software, layer height, wall layers, roof/floor layer, total layers, build orientation, and print temperature.6,8,10–14 These print parameters can have a significant impact on the structural and failure properties of a 3D printed specimen. Careful selection and optimization of these parameters can help to achieve the desired mechanical properties and performance of the printed part.

Materials and 3D printers

Research was conducted utilizing two different 3D printers and three different materials. The Stratasys F170 (Stratasys, Inc., Israel) was used to create specimens in ABS-CF10, and the Markforged Mark Two (Markforged, Inc., Massachusetts) was used to create specimens in Onyx and Onyx with carbon fiber continuous fiber reinforcement.

The manufacturers have provided the following brief descriptions of their materials:

  • ABS-CF10: “Stratasys ABS-CF10 combines standard ABS material with 10% chopped carbon fibre by weight. The result is a low moisture-sensitive FDM® thermoplastic 50% stiffer and 15% stronger than standard ABS 3D printing material.”15

  • Onyx: “Onyx is a micro carbon fibre filled nylon. It's 1.4 times stronger and stiffer than ABS and can be reinforced with any continuous fibre.”16

  • Carbon fiber continuous fiber reinforcement: “Carbon fiber has the highest strength-to-weight ratio of our reinforcing fibres. Six times stronger and eighteen times stiffer than Onyx.”16

Material properties provided by the manufacturers are shown in Table 1.

Table 1.

Manufacturer-Provided Material Properties

Material properties
Printer Material Tensile strength Tensile modulus
Stratasys F170 ABS-CF10 37.7 MPa 3.34 GPa
Markforged Mark Two Onyx 40 MPa 2.4 GPa
Markforged Mark Two Onyx+carbon fiber 800 MPa (carbon fiber) 60 GPa (carbon fiber)

Computer-aided design and 3D printing process

3D computer-aided design (CAD) models of dog bone specimens were created in SolidWorks (software; Dassault Systèmes, Massachusetts) for each material. The specimen dimensions were composed according to which standard the manufacturer had conducted their sample research upon to ensure that no geometry variables were present. Specimens in ABS-CF10 on the Stratasys F170 were created in accordance with ASTM D638 (Type I).17 Specimens in Onyx, and Onyx with carbon fiber continuous fiber reinforcement were created in accordance with ASTM D638 (Type IV).17 CAD data were then imported into the manufacturer's slicing software, and the printing parameters chosen were applied. The printing parameters chosen for each specimen are detailed in Table 2.

Table 2.

Specimen Printing Parameters

Parameters
Printer+material Fill density+reinforcement fill pattern Nozzle temperature Layer/fiber orientation Software Layer height Wall layers Roof/floor layers Total fiber layers Total layers Build orientation
Stratasys F170—ABS-CF10 100% 270°C ±45 Grab CAD 0.254 mm 1 1/1 N/A 75 XZ
Markforged Mark Two—Onyx 100% 275°C ±45 Eiger 0.125 mm 2 4/4 N/A 26 XY
Markforged Mark Two—Onyx+Carbon Fiber 100% (isotropic reinforcement pattern) 275°C Onyx: ±45 Carbon Fiber: 0 Eiger 0.125 mm 2 4/4 8 26 XY

N/A, not applicable.

Five specimens per material were created, meeting the requirement of ISO 527-1 testing procedure.18 Once printed, each specimen was measured using an Axiom too CMM (Aberlink Ltd., Gloucestershire, UK) (last calibration January 2023) across width and depth to obtain cross-sectional area and to analyze accuracy up to 2.4 μm.

Mechanical testing

Mechanical tensile tests were conducted using a ZwickRoell Z030 (ZwickRoell Ltd., Worcestershire, UK) material testing machine (last calibration June 2022), with a load cell of 10 KN. The testing speeds were replicated from the manufacturers' testing procedures: 2 mm/min for the ABS-CF10 and 2.54 mm/min for the Onyx and Onyx with carbon fiber. Test results were recorded, and data graphs were plotted using Microsoft Excel (software; Microsoft, Washington). A Dantec Dynamics digital image correlation (DIC) (Dantec Dynamics, Denmark) system was used during the mechanical testing to measure the strain distribution on the surface of the entire sample.

DIC is an optical method used to measure the deformation or strain of a material by analyzing images of the material's surface before and after deformation by tracking a speckle pattern. Using DIC in conjunction with tensile testing provides a more detailed and accurate understanding of the material's mechanical behaviors as it provides a full-field measurement of longitudinal strain over the entire surface of the specimen. The elastic modulus was calculated from the initial linear portion of the stress–strain curve using force data from the ZwickRoell Z030 and strain data from the DIC.

Microscopy

Visual inspection of the test samples was conducted using a Keyence VHX-5000 digital microscope (Keyence Ltd., Milton Keynes, UK). This allowed for detailed visualization of the microstructure of the material and the print quality at a high resolution. It also provided information on the fiber–matrix interface, the distribution, size, and orientation of fibers, and any defects within the printed specimen.

Results and Discussion

Dimensional accuracy

The width and depth measurements of each specimen were measured using the Axiom too CMM to verify the cross-sectional area and to evaluate the dimensional accuracy achieved by each 3D printer.

Mean and standard deviation values for each specimen were calculated, as well as an unpaired Student's t-test was performed to compare the CMM-measured dimensions with the nominal dimensions. A p-value of <0.05 indicates that a statistically significant difference exists. The p-value result received is consistent with other studies evaluating the dimensional accuracy of 3D printed tensile specimens8,19 and can be seen in Tables 3 and 4. These results show that there is strong evidence to suggest that there is a real difference between the nominal and CMM-measured values, and it is unlikely that this difference was due to chance or random variability alone, therefore indicating that the samples did not conform to the expected dimensions The deviation of a 3D printed component from the original CAD data is important information for designers and engineers to understand so they can account for this when designing and manufacturing their 3D printed components.

Table 3.

Sample Width Measurement

Sample width measurement (mm)
Material sample Nominal Measured average SD % Error p
Stratasys F170—CF10 13.00 13.18 0.03 1.38% <0.001
Markforged Mark Two—Onyx 6 6.22 0.05 3.67% <0.001
Markforged Mark Two—Onyx+eight layers of Carbon Fiber at 0 degree 6 6.26 0.04 4.33% <0.001

SD, standard deviation.

Table 4.

Sample Depth Measurement

Sample depth measurement (mm)
Material sample Nominal Measured average SD % Error p
Stratasys F170—CF10 3.2 3.27 0.01 2.19% <0.001
Markforged Mark Two—Onyx 3.2 3.36 0.02 5% <0.001
Markforged Mark Two—Onyx+eight layers of Carbon Fiber at 0 degree 3.2 3.42 0.03 6.88% <0.001

Tensile test and DIC

The mechanical properties studied from the tensile test results are ultimate tensile strength, strain at break, and elastic modulus. Across the three materials studied, two materials outperformed the manufacturer-supplied values for tensile strength, whereas one material was below the manufacturer's value. The DIC results show larges variances in strain across all specimens and materials. This is due to a combination of printing defects, fiber orientations, and the inhomogeneous material properties.

Stratasys F170—ABS-CF10

The manufacturer-given data for the tensile strength of ABS-CF10 is 37.7 MPa.15 On average, the tensile test results achieved in this research were 33.04 MPa (See Figure 1); this gave a percentage difference of −12.36% from the stated manufacturer's value. The standard deviation across the five samples was 0.34 MPa, with the highest tensile strength recorded being 33.58 MPa, which is 10.93% below the manufacturer's value. The average strain at break recorded across the five samples was 2.47%, compared with 2.7% stated by the manufacturer. The average elastic modulus across the five samples was 3.44 GPa, and the manufacturer-stated value is 3.34 GPa. The DIC data used for two of the ABS-CF10 samples are shown in Figure 2. The break point was consistent across the five samples with the break at the start of the gauge length; this break point is consistent with other studies evaluating tensile strength of 3D printed specimens.8,20

FIG. 1.

FIG. 1.

ABS-CF10 tensile test results.

FIG. 2.

FIG. 2.

ABS-CF10 DIC data. DIC, digital image correlation.

The samples were built following Stratasys' build document21 regarding specimen standard, build orientation, and layer height. Stratasys conducted their ABS-CF10 material testing on the Stratasys F370 and used Insight software (Stratasys) to control printing parameters and slicing. Insight offers more control over printing parameters such as seam control, which was not available when preparing samples to print on the F170 using GrabCAD (software; GrabCAD, Massachusetts) Print software. Research has shown that seam control does not have a significant impact on the structural properties of the samples.22,23 Results from visual inspection work carried out on the ABS-CF10 samples are shown in Figure 3.

FIG. 3.

FIG. 3.

(a) Cross section of ABS-CF10 filament × 150 magnification. (b) ABS-CF10 specimen cross section × 150 magnification. (c) ABS-CF10 specimen cross section × 100 magnification. (d) ABS-CF10 specimen cross section × 200 magnification.

A sample of ABS-CF10 filament and tensile specimen was selected for analysis. Carbon fibers can be seen embedded in the ABS matrix (Fig. 3a); images in Figure 3b–d taken at the fracture surface show several defects including poor layer adhesion (1), leading to voids in the internal structure of the sample; interbead voids can be seen between layers (2); along with fiber pullout at the fracture surface and associated cavities (3). The large void shown in the top of Figure 3c is due to the 45° infill pattern used during slicing and lead to the weakest point in the cross section of the specimen. Histogram image analysis, using the distribution of pixel intensities from the microscopy images, was used to determine the volume fraction through the cross section of the broken specimens. The average volume fraction of the specimens was 9.85%, which is slightly lower than the 10% stated by the manufacturer.15

The density of the ACF10 material used in this research was calculated as 1.07 g/cm3. This was 0.02 g/cm3 less than the reported density of 1.09 g/cm3.15,24 The average density of the CF10 specimens produced on the F170 was 1.02 g/cm3. The resultant density of the printed samples was 95.33% of the density of the material itself. This shows that there is a 4.67% void content in the samples.

The results of microscopy and density analysis, combined with lower-than-expected tensile test results, determine that the fibers within the ABS-CF10 specimen are not properly wetted with the matrix. This has resulted in the formation of large voids within the specimen and weak interfacial bonding. This weak interfacial bonding has led to the load transfer between the matrix and fiber being limited, resulting in a weaker composite than anticipated, and therefore resulting in fiber pullout and the lower-than-expected mechanical properties. The lower-than-expected volume fraction of the specimens also has an impact on the mechanical properties being lower than stated by the manufacturer, as more of the specimen is made up of the matrix material, which has lower mechanical properties than the carbon fiber.

Markforged Mark Two—Onyx

The manufacturer-given data for the tensile strength of Onyx is 40.64 MPa.16 On average, the tensile test results achieved in this research were 44.17 MPa (see Figure 4); this gave a percentage difference of +8.66% from the stated manufacturers' value. The standard deviation across the five samples was 0.7 MPa, with the highest tensile strength recorded being 44.92 MPa, which is 10.5% above the manufacturer's value. The average strain at break recorded across the five samples was 26% compared with 25% stated by the manufacturer.

FIG. 4.

FIG. 4.

Onyx tensile test results.

The average elastic modulus across the five samples was 1.01 GPa, and the manufacturer's value in their technical report for the same build parameters is 0.91 GPa. The DIC data used for two of the Onyx samples are shown in Figure 5. The break point was consistent across the five samples with the break at the start of the gauge length; this break point is consistent with other studies evaluating tensile strength of 3D printed specimens.8,20 The test samples were manufactured to the specifications in the Markforged material testing technical report25 and printed utilizing the same printer, the Markforged Mark Two. Results from visual inspection work carried out on the Onyx samples are shown in Figure 6.

FIG. 5.

FIG. 5.

Onyx DIC data.

FIG. 6.

FIG. 6.

(a) Cross section of Onyx filament × 150 magnification. (b) Onyx specimen cross section × 150 magnification. (c) Onyx specimen cross section × 200 magnification. (d) Onyx specimen cross section × 200 magnification.

A sample of Onyx filament and tensile specimen was selected for analysis. Carbon fibers can be seen embedded in the nylon matrix (Fig. 6a), images in Figure 6b–d taken at the fracture surface show fiber pullout (3), in addition to clear uniform interbead voids between the layers (2). Significant voids in the print can be seen in Figure 6d (1). Histogram image analysis was used to determine the volume fraction through the cross section of the broken specimens. The average volume fraction of the specimens was 34.89%, which is consistent with other research evaluating the volume fraction of Onyx.26

The density of the Onyx material used in this research was calculated as 1.14 g/cm3. This was 0.06 g/cm3 less than the reported density of 1.2 g/cm.3,16,27 The average density of the Onyx specimens produced was 1.02 g/cm3. The resultant density of the printed samples was 89.47% of the density of the material itself. This shows that there is a 10.53% void content in the samples, and this result is consistent with other research investigating the void content of 3D printed samples in Onyx, which range between 7% and 11%.28,29

Microscopy analysis and mechanical test results achieved indicate good print quality. The microscopy analysis showed good layer adhesion, small interbead voids, and no visible signs of defects such as warping, layer shifting, or stringing. Visual inspection of the specimens showed evenly distributed fibers that were bonded well with the matrix, and no large voids or cracks therefore indicating proper wetting. The increase of mechanical properties observed shows that there was good adhesion and load transfer between the fibers and matrix, also indicating that the fibers are properly wetted with the matrix. Good quality control measures were followed including a brand-new reel of filament ensuring no degradation to the material had occurred, a new print nozzle, and machine calibration. The combination of good print quality, proper wetting, and quality control measures explains why the mechanical properties exceeded expectation.

Markforged Mark Two—Onyx+carbon fiber

The manufacturer-given data for the tensile strength of Onyx with eight layers of carbon fiber, built in their technical report,25 are 106.8 MPa. On average, the tensile test results achieved in this research were 123.15 MPa (see Figure 7); this gave a percentage difference of +15.31% from the stated manufacturer's results in their technical report. The standard deviation across the five samples was 8.71 MPa, with the highest tensile strength recorded being 135.61 MPa, which is 26.98% above the manufacturer's results in their technical report. The average strain at break recorded across the five samples was 1.65% compared with 1.5% stated by the manufacturer. All five samples of Onyx with eight layers of carbon fiber in this build orientation yielded too quickly to be able to calculate elastic modulus from the initial linear portion of the stress–strain curve. These results are consistent with the manufacturer's technical report.25 The break point was consistent across the five samples with the break at the start of the gauge length; this break point is consistent with other studies evaluating tensile strength of 3D printed specimens.8,20

FIG. 7.

FIG. 7.

Onyx + carbon fiber tensile test results.

The test samples were manufactured to the specifications in the Markforged material testing technical report25 and printed utilizing the same printer, the Markforged Mark Two. The test samples yield strength had a standard deviation of 8.71 MPa, which is the largest across the material tests conducted, indicating that Onyx with added continuous strands of carbon fiber is less repeatable and less consistent than 3D printed material containing only chopped strand of carbon fiber; however, adding continuous strands of carbon fiber can provide significantly higher tensile strength. The stress–strain graph shows multiple drops in stress in the specimen toward the end of the test before the final break.

These drops represent when individual strands of the continuous carbon fibers broke within the specimen before its final break. The presence of two linear portions on the graph indicates that Onyx+Carbon Fiber specimen has two different phases that respond differently to stress and have different stiffnesses. The stiffness of the material reduces after the fibers stop taking effect. This is explained due to each of its constituent materials having different material properties. When the first linear portion of the graph concludes, permanent damage has occurred to the specimen, although it is way below its final break. Results from visual inspection work carried out on the Onyx+Carbon Fiber samples are shown in Figure 8.

FIG. 8.

FIG. 8.

(a) Onyx+Carbon Fiber specimen cross section × 50 magnification. (b) ONYX+Carbon Fiber specimen cross section × 200 magnification.

An Onyx+Carbon Fiber tensile specimen was selected for analysis. The transition from the central core of Onyx to Onyx+Carbon Fiber layers can be clearly seen (Fig. 8a); the addition of the continuous strand of carbon fiber has resulted in less compact Onyx layers that surround the eight layers of carbon fiber leading to larger interbead voids. Clear fiber pullout can be seen on the continuous strand of carbon fiber section of the sample (3). Voids can also be seen throughout the sample (1).

The density of the carbon fiber material used in this research was calculated as 1.33 g/cm3. This was 0.13 g/cm3 more than the reported density of 1.2 g/cm3 by Markforged, yet it was 0.07 g/cm3 less than the reported density of 1.4 g/cm3 found in the academic literature.27 Due to the printing parameters, the density of the Onyx+Carbon Fiber specimens should theoretically be 1.2 g/cm3. The average density of the printed Onyx+Carbon Fiber specimens produced was 1.14 g/cm3. The resultant density of the printed samples was 95% of the density of the material make up. This shows that there is a 5% void content in the samples, which is lower than results found from other research investigating the void content of 3D printed samples in Onyx with continuous carbon fiber reinforcement that ranges between 7% and 11%.28,29

The microscopy results show that the Onyx sections have good layer adhesion and compaction, with an even surface finish with small voids throughout the print indicating good print quality. The density analysis of the specimens also indicates good print quality. Good quality control measures were followed including a brand-new reel of filament ensuring no degradation to the material had occurred, a new print nozzle, and machine calibration. The combination of the carbon fiber material having a higher density than that stated by Markforged, good quality control measures, and the microscopy and density results showing that the print has a low void content of 5% explains why the tensile test results achieved are higher than that stated by Markforged.

Conclusions

Three different composite 3D printing materials were analyzed in this study, utilizing two different 3D printers. Build documents were followed to create test samples, and tensile tests were then performed with DIC and analyzed to give mechanical properties. Data extracted from the tensile tests were analyzed against material properties given by the manufacturers. This study shows inconsistencies between material properties stated by the manufacturers and those achieved by users. These inconsistencies illustrate that designers and engineers cannot rely solely on manufacturer's data sheets for AM components, and testing validation should always be performed.

Stratasys' ABS-CF10 was unable to meet the manufacturer's tensile strength value by 12.36%. Markforged Onyx and Onyx+carbon fiber continuous reinforcement exceeded the manufacturer's values by 8.66%, and 15.31%, respectively. While Onyx+Carbon Fiber had the largest percentage increase on tensile strength, it measured the lowest dimensional accuracy and repeatability. Microscopy and density measurement were used to analyze print quality, defects, volume fraction, and fiber–matrix wetting to determine what influenced the mechanical properties of the specimens. Poor fiber–matrix wetting, large voids, and weak interfacial bonding were attributed to the ABS-CF10 material not reaching the manufacturer's values. While good print quality, low void percentage, proper fiber–matrix wetting, and good control measures were attributed to the Onyx and Onyx+Carbon Fiber specimens exceeding the manufacturer's values.

Further research is necessary into the discrepancies that could exist between individual printers of the same model. A comparative study that investigates how individual printers of the same model, with the same material, and the same build file can differ will enable an analysis of the repeatability within 3D printer models.

Authors' Contributions

A.B.: Conceptualization, methodology, software, validation, formal analysis, investigation, writing—original draft (lead), visualization. R.G.: Conceptualization, methodology, software, validation, formal analysis, investigation, writing—original draft. B.D.: Writing—review and editing. P.S.: Methodology, writing—review and editing.

Author Disclosure Statement

No competing financial interests exist.

Funding Information

No funding was received for this article.

References

  • 1. Russo AC, Andreassi G, Di Girolamo A, et al. FDM 3D printing of high performance composite materials. In: 2019. II Workshop on Metrology for Industry 40 and IoT (MetroInd4 0&IoT); 2019; pp.355–359. [Google Scholar]
  • 2. McAlpine M. 3D printing functional composites & devices. In: Proceedings of the Composites at Lake Louise 2019, 2019 Nov 10–14; Alberta, Canada. New York: ECI 2019. (Kieffer J, Spoeke E, Shofner M. eds.) Alberta, Canada; 2019. [Google Scholar]
  • 3. Blok LG, Longana ML, Yu H, et al. An investigation into 3D printing of fibre reinforced thermoplastic composites. Addit Manuf 2018;22:176–186. [Google Scholar]
  • 4. Markforged. 3D Printing Carbon Fiber and Other Composites. Massachusetts; 2023. Available from: https://markforged.com/resources/learn/design-for-additive-manufacturing-plastics-composites [Last accessed: April 25, 2023].
  • 5. Hu Y. 3D printed FDM composites: fabrication, microstructure and properties (Doctoral dissertation, RMIT University); 2022. [Google Scholar]
  • 6. Hodzic D, Pandzic A.. Influence of carbon fibers on mechanical properties of materials in FDM technology. In: Proceedings of the 30th DAAAM International Symposium on Intelligent Manufacturing and Automation, Zadar, ISSN 2019. Oct; pp.1726–9679. [Google Scholar]
  • 7. Naranjo-Lozada J, Ahuett-Garza H, Orta-Castañón P, et al. Tensile properties and failure behavior of chopped and continuous carbon fiber composites produced by additive manufacturing. Addit Manuf 2019;26:227–241. [Google Scholar]
  • 8. González-Estrada OA, Pertuz A, Quiroga Mendez JE. Evaluation of tensile properties and damage of continuous fibre reinforced 3D-printed parts. Key Eng Mater 2018;774:161–166. [Google Scholar]
  • 9. Sanei SHR, Popescu D. 3D-printed carbon fiber reinforced polymer composites: A systematic review. J Compos Sci 2020;4(3):98. [Google Scholar]
  • 10. Yavas D, Zhang Z, Liu Q, et al. Fracture behavior of 3D printed carbon fiber-reinforced polymer composites. Compos Sci Technol 2021;208:108741; doi: 10.1016/j.compscitech.2021.108741 [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 11. Torrado AR, Roberson DA. Failure analysis and anisotropy evaluation of 3D-printed tensile test specimens of different geometries and print raster patterns. J Failure Anal Prev 2016;16(1):154–164. [Google Scholar]
  • 12. Van Der Klift F, Koga Y, Todoroki A, et al. 3D printing of continuous carbon fibre reinforced thermo-plastic (CFRTP) tensile test specimens. Open J Compos Mater 2016;6(01):18. [Google Scholar]
  • 13. Todoroki A, Oasada T, Mizutani Y, et al. Tensile-test-property evaluations of 3D printed continuous carbon fiber reinforced thermoplastic composites. J Japan Soc Compos Mater 2019;45(4):141–148; doi: 10.6089/jscm.45.141 [DOI] [Google Scholar]
  • 14. Hoshikawa Y, Shirasu K, Tsuyuki J, et al. Experimental and numerical evaluation of open hole tensile properties of 3D printed continuous carbon fiber reinforced thermoplastics. Mater Syst 2021;38:49–54; doi: 10.34401/materialssystem.38.0_49 [DOI] [Google Scholar]
  • 15. Stratasys. ABS-CF10 Data Sheet. 2021. Available from: https://www.stratasys.com/contentassets/91f958a377d441488d273384663390dd/mds_fdm_abs-cf10_0222a.pdf?v=49aec5 [Last accessed: April 25, 2023].
  • 16. Markforged. Material Datasheet. 2021. Available from: https://www-objects.markforged.com/craft/materials/CompositesV5.2.pdf [Last accessed: April 25, 2023].
  • 17. International A. ASTM Designation: D638-14. 2014. Available from: https://www.astm.org/d0638-14.html [Last accessed: March 2, 2023].
  • 18. Institution BS. BS EN ISO 527-1:2019. 2019. Available from: https://www.iso.org/standard/75824.html#:∼:text=1.1%20This%20document%20specifies%20the,subsequent%20parts%20of%20ISO%20527 [Last accessed: March 2, 2023].
  • 19. Pyl L, Kalteremidou K-A, Van Hemelrijck D. Exploration of specimen geometry and tab configuration for tensile testing exploiting the potential of 3D printing freeform shape continuous carbon fibre-reinforced nylon matrix composites. Polym Test 2018;71:318–328. [Google Scholar]
  • 20. Melenka GW, Schofield JS, Dawson MR, et al. Evaluation of dimensional accuracy and material properties of the MakerBot 3D desktop printer. Rapid Prototyp J 2015;21(5):618–627. [Google Scholar]
  • 21. Stratasys. Materials Testing Procedure. 2021. Available from: https://www.stratasys.com/siteassets/materials/materials-catalog/fdm-materials/antero-840cn03/BR_FDM_MaterialsTestingProcedure_0121a.pdf?v=4a0149 [Last accessed: April 23, 2023].
  • 22. Auffray L, Gouge P-A, Hattali L. Design of experiment analysis on tensile properties of PLA samples produced by fused filament fabrication. Int J Adv Manuf Technol 2022;1–15. [Google Scholar]
  • 23. Sardinha M, Frutuoso N, Vicente CMS, et al. Influence of seams in the mechanical properties of PLA produced with multiple extrusion modules. Proc Struct Integr 2020;28:358–363. [Google Scholar]
  • 24. Xu J, Gao M, Zhan J, et al. Towards support-free design for 3D printing of thin-walled composite based on stratified manufacturability reinforcement. CIRP J Manuf Sci Technol 2022;38:457–472. [Google Scholar]
  • 25. Morgan RV, McReynolds B, Husmann K, et al. Markforged Continuous Fiber Composite Material Testing. Los Alamos National Lab.(LANL): Los Alamos, NM (United States); New Mexico; 2020. [Google Scholar]
  • 26. Saeed K, McIlhagger A, Harkin-Jones E, et al. Characterization of continuous carbon fibre reinforced 3D printed polymer composites with varying fibre volume fractions. Compos Struct 2022;282:115033. [Google Scholar]
  • 27. Jayashankar DK, Devarajan A, Dong G, et al. Design and manufacture of a continuous fiber-reinforced 3D printed unmanned aerial vehicle win. In: 2021. International Solid Freeform Fabrication Symposium 2021. University of Texas at Austin. [Google Scholar]
  • 28. Papa I, Silvestri AT, Ricciardi MR, et al. Effect of fibre orientation on novel continuous 3d-printed fibre-reinforced composites. Polymers 2021;13(15):2524. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 29. Ueda M, Kishimoto S, Yamawaki M, et al. 3D compaction printing of a continuous carbon fiber reinforced thermoplastic. Compos Part A Appl Sci Manuf 2020;137:105985. [Google Scholar]

Articles from 3D Printing and Additive Manufacturing are provided here courtesy of SAGE Publications

RESOURCES