Skip to main content
. 2025 Feb 19;10(8):7683–7696. doi: 10.1021/acsomega.4c07195

Table 2. Geopolymer with Different Materials Contaminated by Cesiuma.

material SSA origin saturated (MPa)
unsaturated (MPa)
    5% 8% 10% 5% 8% 10%
    SSA 10%          
AC BA 14.87 ± 0.6 12.38 ± 0.6 11.68 ± 0.6 14.37 ± 0.6 11.68 ± 0.6 10.58 ± 0.6
  BP 14.42 ± 0.6 12.53 ± 0.6 10.98 ± 0.6 13.68 ± 0.6 12.03 ± 0.6 10.23 ± 0.6
IER BA 14.47 ± 0.6 11.98 ± 0.6 12.03 ± 0.6 14.08 ± 0.6 11.33 ± 0.6 10.83 ± 0.6
  BP 14.57 ± 0.6 11.93 ± 0.6 11.93 ± 0.6 13.93 ± 0.6 11.53 ± 0.6 10.53 ± 0.6
    SSA 30%          
AC BA 14.32 ± 0.4 11.25 ± 0.4 10.87 ± 0.4 11.83 ± 0.4 10.11 ± 0.4 9.85 ± 0.4
  BP 13.68 ± 0.4 11.36 ± 0.4 10.91 ± 0.4 11.70 ± 0.4 10.26 ± 0.4 9.57 ± 0.4
IER BA 13.35 ± 0.4 11.74 ± 0.4 10.65 ± 0.4 11.40 ± 0.4 10.49 ± 0.4 9.65 ± 0.4
  BP 13.25 ± 0.4 11.52 ± 0.4 10.33 ± 0.4 11.08 ± 0.4 10.69 ± 0.4 9.87 ± 0.4
    SSA 50%          
AC BA 9.32 ± 0.4 9.25 ± 0.4 9.87 ± 0.4 8.83 ± 0.4 8.11 ± 0.4 7.85 ± 0.4
  BP 8.68 ± 0.4 9.36 ± 0.4 8.91 ± 0.4 7.70 ± 0.4 8.26 ± 0.4 7.57 ± 0.4
IER BA 8.35 ± 0.4 8.74 ± 0.4 9.65 ± 0.4 8.40 ± 0.4 7.49 ± 0.4 6.65 ± 0.4
  BP 8.25 ± 0.4 8.52 ± 0.4 8.33 ± 0.4 7.08 ± 0.4 7.69 ± 0.4 6.87 ± 0.4
a

The columns designated as 5%, 8%, and 10% indicate the quantity of activated carbon (AC) or ion exchange resin (IER) employed in the experiment.