Abstract

Hydrogen produced with no greenhouse gas emissions is termed “green hydrogen” and will be essential to reaching decarbonization targets set forth by nearly every country as per the Paris Agreement. Proton exchange membrane water electrolyzers (PEMWEs) are expected to contribute substantially to the green hydrogen market. However, PEMWE market penetration is insignificant, accounting for less than a gigawatt of global capacity. Achieving substantive decarbonization via green hydrogen will require PEMWEs to reach capacities of hundreds of gigawatts by 2030. This paper serves as an overarching roadmap for cell-level improvements necessary for gigawatt-scale PEMWE deployment, with insights from three well-established hydrogen technology companies included. Analyses will be presented for economies of scale, renewable energy prices, government policies, accelerated stress tests, and component-specific improvements.
1. Introduction
Nearly every country has joined the landmark Paris Agreement to achieve global net zero emissions by 2050. Hydrogen will be essential to reach these targets as it can mitigate emissions for sectors without promising decarbonization solutions, such as grid-scale energy storage, long-haul transportation, and industrial manufacturing.1,2 It can be used electrochemically to generate electricity or as a chemical feedstock to produce commodities such as steel, cement, ammonia, and other valued chemicals.3 Since hydrogen usage does not generate greenhouse gases (GHGs), as long as the energy used to produce hydrogen comes from clean power sources (e.g., solar, wind, geothermal, and nuclear), the hydrogen can be deemed “green.”
A proton exchange membrane water electrolyzer (PEMWE) is a promising green hydrogen technology that utilizes electricity to split water into oxygen and hydrogen. When paired with clean power sources, PEMWEs can mass-produce green hydrogen and are expected to make up 40% of the green hydrogen market, with the remaining 60% comprised of alkaline and solid oxide electrolyzers.4 However, market penetration of green hydrogen is insignificant compared to hydrogen generated from GHG-intensive methods due to higher production costs ($1.0–$2.5/kg vs. $4.0–$9.0/kg).5 As of 2022, global green hydrogen capacity was 11 gigawatts (one gigawatt, or GW, can produce ∼500 tons of hydrogen daily6),7 with PEMWEs making up only 0.3 GW. To achieve net zero emissions by 2050, it is projected that PEMWE capacity will need to reach 220 GW by 2030 and 1130 GW by 2050.4
1.1. PEMWE Overview
Three types of water electrolyzers are expected to make up the green hydrogen market: alkaline, solid oxide, and proton exchange membrane (PEM). While alkaline water electrolyzers—characterized by having two electrodes operating in a liquid alkaline electrolyte—have become fully commercialized, their inability to operate under highly dynamic loads and at high current densities and pressures restricts their potential for large-scale hydrogen production.8,9 Solid oxide water electrolyzers—characterized by high operating temperatures (>500 °C) and the use of a ceramic electrolyte—are highly efficient and may hold promise; however, their developmental stage is still early,9 with only a handful of companies selling them. We refer the reader to the literature for detailed analyses of the different water electrolyzer types.8−12 PEM water electrolyzers (PEMWEs) possess several characteristics that make them suitable for widespread green hydrogen production: high efficiencies, long lifetimes, large range of operational current densities (up to 3 A·cm–2),13,14 fast dynamic response times, and the ability to operate at differential pressure.9
A generic schematic of a PEMWE cell is shown in Figure 1. Liquid water is fed into the anode side, where the oxygen evolution reaction (OER) occurs, generating oxygen gas bubbles, electrons, and protons. The oxygen exits the cell while the electrons and protons (which carry water via electro-osmotic drag)15 travel—via current collectors and the membrane, respectively—to combine at the cathode, where the hydrogen evolution reaction (HER) occurs to generate hydrogen gas.
Figure 1.
Generic schematic of a proton exchange membrane water electrolyzer (PEMWE).
A PEMWE cell consists of a proton exchange membrane, two catalyst layers, two transport layers, and two separator plates. The proton exchange membrane (∼100 μm)16 is responsible for maximizing proton conductivity while compartmentalizing the oxygen gas to the anode and hydrogen gas to the cathode. Since gas permeability is inversely correlated with proton conductivity,17 achieving low gas permeability while keeping conductivity high is a central research challenge. The membrane is sandwiched between two catalyst layers (∼1–10 μm),18 which serve as the electrodes of the system—typically consisting of an iridium-based catalyst for the anode and a platinum-based catalyst for the cathode.8 Outside each catalyst layer are diffusion layers: the gas diffusion layer (GDL, ∼100–300 μm)19 on the cathode side and the porous transport layer (PTL, ∼250–500 μm)20 on the anode side. The GDL is primarily responsible for gaseous transport (hydrogen gas out), while the PTL is responsible for liquid and gaseous transport (liquid water in; oxygen gas out). Both the PTL and GDL require establishing electronic conduction with the adjacent catalyst layer, but the PTL is subject to much higher redox potentials, imposing material limitations.8 The last component on each side of the cell is the separator plate (∼1.5 mm),21 which contains flow fields to distribute reactants (water) and remove products (oxygen and hydrogen gas).22 Please note that in a stack, numerous cells are combined in series, so separator plates will contain flow fields on both sides (unless they are located at the ends). Thus, due to their two-sided nature, separator plates are also called bipolar plates (BPPs). Commercial stacks contain many cells (∼30–200),23,24 each with active areas of ∼1000–3000 cm2, with total power capacities currently around 500 kW–3 MW.
Although PEMWEs are predominantly used to produce hydrogen, the oxygen generated also has valuable uses.25 Interestingly, some PEMWE designs are even specialized for oxygen production.26 The oxygen can be used in medicine (heart/lung disease patients), defense (fighter aircraft and submarines), spacecraft (life support27), and industry (food processing, welding, metallurgy, semiconductors), among other applications. In any case, safe handling of hydrogen and oxygen is necessary as mixtures present an explosive hazard. Often, hydrogen is diluted with air or inert gases (such as nitrogen) and released into the atmosphere to prevent ignition. Alternatively, the hydrogen can be circulated to a fuel cell system to feed power back to the electrolyzer, increasing overall system efficiency.27
1.2. Configuration Variations
Conventional operation is characterized by pressures of ∼30 bar and temperatures of 50–90 °C.9 PEMWE pressure is typically defined by hydrogen pressure, as the oxygen is usually vented upon generation (and thus is at ambient pressure). Pressure is generated directly from hydrogen gas being produced, assuming the membrane can withstand any associated mechanical stress.29 This so-called “differential pressure” operation provides benefits over isobaric operation because less downstream mechanical compression will be required for end usage. However, increased pressure comes greater hydrogen crossover into the oxygen-rich anode, resulting in serious ignition concerns. Only a 4% volume of hydrogen in oxygen would form an ignitable safety hazard (i.e., 4% is the lower explosive limit, or LEL).30 Thus, given these safety considerations, state-of-the-art PEMWEs do not exceed 50 bar. However, as discussed in the next paragraph, there is considerable potential to operate at much higher pressures. Regarding temperature, higher operating temperatures lead to voltage efficiency improvements.31 In conventional operation, heat is supplied to the cell and produced by electrochemical losses to maintain a temperature of 50–90 °C. However, increasing temperatures above the boiling point of water poses a unique set of challenges as 1) state-of-the-art membranes (i.e., PFSA membranes) rely on liquid-water-assisted proton conduction, and 2) vapor-fed operation is not well studied.32 Potential strategies to enable high-temperature operation will also be discussed in this section.
High-pressure operation is an attractive alternative to conventional operation as substantial pressurization or liquefaction of hydrogen is required for many end uses: 200 bar for gaseous storage, ∼300 bar for the Haber–Bosch process, 350 bar for heavy-duty fuel cell vehicles, and 700 bar for passenger fuel cell vehicles.33 Since hydrogen is typically produced at 30 bar, adjusting the electrolyzer to output at greater pressures could reduce equipment count, process complexity, capital costs, and maintenance costs, all while lowering the energy required to perform the final compressive steps.33 In the literature, high-purity hydrogen at differential pressures up to 350 bar has been shown.34 However, gas crossover issues that already exist in conventional operation are exacerbated under higher pressures.33 Strategies for mitigating crossover will be discussed in Section 4.3.3.
Higher operating temperatures result in a lower reversible cell potential (e.g., 1.14 V at 200 °C versus 1.23 V at 20 °C35) and lower kinetic overpotentials.32 However, increased component corrosion (e.g., BPPs and PTLs) and decreased proton conductivity (due to membrane dehydration) could also result.31 Thus, corrosive-resistant materials need to be implemented and strategies to ensure proton conductivity need to be developed—such as incorporating organic fillers into the membrane (to enhance water uptake)36−42 or increasing the water pressure at the anode.31
Lastly, novel configurations are also possible and can lead to performance improvements. One design by Hystar43 changes the water inlet from the anode to the cathode and adds airflow to the anode. With these changes, Hystar claims that membrane thickness can be reduced by ∼85% (from state-of-the-art 125 μm to 20 μm) since any crossover hydrogen (i.e., hydrogen in the anode) will be diluted with the anode air feed, mitigating the risk of forming an ignitable gas mixture. Such thin membranes could reduce ohmic losses and increase voltage efficiency substantially, as ohmic overpotentials currently comprise a significant portion of voltage losses (∼40% at a typical operating current density of 2 A·cm–2).18 However, several challenges must be addressed, including removing N2/CO2 contaminants (which travel via diffusion from the anode) in the hydrogen outlet.
1.3. Motivation
PEMWEs will require cost and performance improvements to economically compete against conventional forms of hydrogen production.5 The roadmap for GW-scale deployment is complex, but this paper will capture many considerations: deployment targets, government policies, production/capital costs, economies of scale, component-specific improvements, durability testing, and safety regulations. Please note that this paper will focus on cell-level components instead of stack and balance of plant aspects. Two factors distinguish this review from others: 1) broader economic and political considerations will be discussed along with scientific research goals, and 2) less focus will be put on the current state of PEMWEs (for such reviews, please refer to the literature5,8,18,46−48), but instead on improvements necessary to reach GW-scale deployment.
This paper will be presented as follows: first, global green hydrogen policies will be overviewed to orient the reader to the current hydrogen landscape. Then, targets for PEMWE capital costs and hydrogen production costs will be outlined. Next, component-specific research will be discussed in the context of cost, efficiency, and durability improvements. Afterward, durability testing protocols (i.e., accelerated stress tests) will be proposed for each component. Penultimately, we will zoom out and have three industrial companies—NEL Hydrogen, Plug Power, and an undisclosed company—offer their unique perspectives on how global efforts can be directed for PEMWE expansion. To conclude, all the insights in this paper will be summarized to present a concise roadmap for GW-scale deployment.
2. Deployment Targets
Global hydrogen demand was 94 million tons (Mt) in 2021, accounting for nearly 2.5% of global energy consumption. Nearly half of this demand went toward refining hydrocarbons (46%), while the rest was directed to the production of ammonia (35%), methanol (15%), and steel (4%; via direct reduction of iron).5 Transport is a small but growing source of demand, on the order of 30,000 tons (0.03% of global demand), corresponding to a 60% increase over the previous year.50 This demand was primarily for fueling trucks, buses, and passenger vehicles, with the potential to expand in the rail, shipping, materials handling (e.g., forklifts), and aviation sectors.
The push to meet hydrogen demand has led to the deployment of MW-scale systems in recent years. Recent deployments include 1) the first floating offshore PEMWE (France), utilizing a 1 MW system from Plug Power,51 and 2) a 1.5 MW load-balancing PEMWE (Germany) that feeds hydrogen directly into a natural gas grid.52 In addition, numerous multi-MW systems can be seen for projects under construction and in the final investment decision (FID) stages.53
2.1. Global Landscape
In recent years, an increasing number of nations have presented hydrogen roadmaps for decarbonization or included hydrogen as part of a larger clean energy strategy. These roadmaps/strategies often entail plans for hydrogen production and/or utilization. Table 1 outlines such policies, ordered by the date of release. This table builds on previous efforts by Wappler et al.54 in 2022 by summarizing documents gathered through Australia’s hydrogen policy tracking resource “HyResource.”55 In a little over a year since Wappler et al. published their analysis, 23 countries have announced hydrogen policies, increasing the total number of nations to 53.
Table 1. Summary of National Hydrogen Policies Sorted by Region and in Chronological Order, Expanded from Ref (54) and Primarily Sourced from HyResource55.
Summary of National Hydrogen Policies Sorted by Region and in Chronological Order

For the hydrogen “type,” several distinctions exist between “green” and “clean” hydrogen (please note, however, that these two terms are sometimes used interchangeably). Clean hydrogen is a more general term to refer to production processes that result in little or no GHG emissions. Thus, clean hydrogen includes green hydrogen but also processes such as “blue” hydrogen, where hydrogen is produced via steam methane reformation (SMR) with carbon capture and underground storage (CCUS). Blue hydrogen (and in some cases, gray hydrogen—or hydrogen produced from SMR without CCUS) is presented as a bridging device to meet short-term demands for hydrogen while green hydrogen technologies gradually become online.112 Short-term demands of clean and green hydrogen include the steel industry of the European Union113 as well as transport fuels for the development of a green hydrogen transport fuel market. In this vein, certification schemes for tracking the GHG emission intensity of hydrogen production are under development, such as with the European Union’s CertifHy114 and Australia’s Guarantee of Origin (GO) scheme.115
When considering the production of green hydrogen from a life cycle analysis (LCA) standpoint, water electrolysis entails the lowest natural resource costs, human health impacts, and ecological impacts when combined with wind or nuclear power (but not with solar photovoltaics, due to their relatively intense environmental impact).116−118 Regarding external cost factors (e.g., human health impacts, ecological impacts, and resource depletion), electrolysis coupled with wind power is one of the most favorable hydrogen production methods, green or otherwise.117 Lastly, in terms of global warming potential, electrolysis is slightly more carbon intensive than biomass gasification with carbon capture (which has the potential to reach net negative CO2-equivalent emissions), although the latter entails far greater emissions of criteria pollutants and thus suffers from higher external cost factors.117,119
2.2. 2030 Targets
Figure 2 displays 2030 targets for deployed electrolyzer capacity, sourced from national policy documents in Table 1. The goals are expressed in equivalent nominal electrolyzer power capacity. When green hydrogen production rates were given instead of capacity, the IEA convention of 50 kWh/kg H2 and an assumed capacity factor of 50% were used to estimate an equivalent capacity.120 While many European countries have released some form of a plan involving green hydrogen, around half are also incorporating some amount of clean hydrogen. In Asia, China and India have also announced dual strategies of green and clean hydrogen production, with green hydrogen amounting to 1 Mt/yr for China and a substantial 5 Mt/yr for India. In South America, Chile, Colombia, and Uruguay seek to leverage their abundant renewable energy resources—especially hydropower121,122—to become net exporters of green hydrogen, with Chile targeting a considerable 25 GW of electrolysis by 2030. Several countries in Africa and the Middle East are scaling up green hydrogen production to be large exporters as well. Countries in these regions are also planning to sustainably produce commodities that are traditionally associated with GHG emissions, with Egypt,123 Namibia,124 and the United Arab Emirates105,125 to export green ammonia, and Morocco to export green methanol and other liquid fuels.126,127
Figure 2.

Stated 2030 targets for electrolyzer capacity sourced from documents in Table 1. Targets are expressed in equivalent nominal electrolyzer power capacity (GW); for documents that use hydrogen production as the metric, the IEA convention of 50 kWh/kg H2 and an assumed capacity factor of 50% was used to estimate an equivalent capacity.
2.3. Active versus Planned Projects
Using the IEA database, electrolyzer deployment projects based on nameplate capacity are examined in Figure 3, with distinction drawn between currently active (or nearly active) and planned projects.120Figure 3a depicts electrolyzer deployment projects that are currently active or will be active in the near future, which include projects that are actively operating, under construction, or up to final investment decision (FID). Figure 3b shows projects that are announced but are still in the early planning stages, i.e., projects that are not up to FID. Between the two scenarios is a large discrepancy in total electrolysis deployment, with only 6.9 GW up to FID, amounting to less than 5% of the announced targets. For PEMWEs, there is 0.3 GW currently in operation and ∼0.4 GW in construction or up to FID, with ∼10 GW in the early planning stages. To meet decarbonization goals set by the IEA, it is projected that ∼80–220 GW of installed PEMWE capacity is required by 2030 (assuming a 40% market share with other electrolyzer technologies).4 Clearly, there is an urgent need to rapidly accelerate PEMWE deployment.
Figure 3.
(a) Electrolyzer projects that are active, undergoing construction, or up to final investment decision (FID). (b) All announced electrolyzer projects. Information sourced from the IEA Hydrogen Production and Infrastructure Projects Database.120
Notably, policy targets alone are not fully indicative of the electrolyzer deployment landscape. While countries such as the United States, Japan, and Saudi Arabia do not have targets that specify green hydrogen production or electrolyzer deployment, there are still appreciable amounts of active electrolyzer systems, with further deployments expected. In some cases, national targets are outstripped by planned deployments; for example, Australia has announced goals of 1 GW of electrolyzer capacity by 2030, however, there is already 11 GW of projects in various planning stages. Lastly, policy targets may also shift over time, largely trending upward in hydrogen production targets with each revision.
3. Cost Targets
The United States Department of Energy (U.S. DOE) announced cost targets of $2/kg H2 by 2026 and $1/kg H2 by 2031 for clean hydrogen. In 2021, hydrogen production costs ranged from $1.0–$2.5/kg H2 with SMR (gray hydrogen), $1.5–$3.0/kg H2 with SMR with CCUS (blue hydrogen), and $4.0–$9.0/kg H2 with electrolysis (green hydrogen).5 A multitude of factors—including gas supply constraints, energy security concerns ignited by the invasion of Ukraine, and the exiting of a global pandemic—led to surging natural gas demand and, consequently, natural gas prices as high as $85–$153/MWh around much of Europe and significant parts of Asia after holding steady in a range of ∼$10–$23/MWh since 2015.128 Thus, for affected regions, gray hydrogen costs skyrocketed to $4.8–$7.8/kg H2 in Europe and $5.3–$8.6/kg H2 in Asia (for comparison, this would equate to $121–$198/MWh and $134–$218/MWh, respectively).129 While natural gas prices may decline to 2015 levels in the next few years, and indeed have already returned to pre-pandemic levels across much of the globe, such volatility highlights the potential for green hydrogen powered by diverse and potentially more reliable renewable energy resources. Furthermore, SMR production of hydrogen is highly sensitive to the cost of natural gas. Gray hydrogen consumes approximately 0.039–0.055 MWhnat gas/kg H2, while blue hydrogen consumes 0.077 MWhnat gas/kg H2.119,130 Thus, during volatile natural gas price swings—as recently experienced in Asia and Europe—the price of SMR-produced hydrogen can increase substantially; for example, if natural gas prices rise from $20/MWh (2015 levels) to $100/MWh (2022 levels), the cost of SMR-produced hydrogen would increase $3.1–$6.2/kg H2 (depending on whether CCUS is used), quickly closing the price gap between gray/blue hydrogen and green hydrogen.
3.1. Cost Factors
3.1.1. Electricity Costs
The ability for green hydrogen to become cost competitive is strongly dependent upon the availability of low-cost electricity.131 However, even with relatively cheap electricity prices of $0.05–$0.06/kWh, the cost of the electricity alone to make green hydrogen would equate to $3/kg H2 (with no consideration for capital or operating expenditures), making it difficult to compete with gray hydrogen (with total costs of $1.0–$2.5/kg H2).132 Nonetheless, thanks to the increasing availability of lower cost renewable electricity from solar and wind power, electricity prices equivalent to $0.02/kWh have been observed, which would enable $1/kg H2 in electricity costs.133 To meet a competitive cost point for green hydrogen, capital expenditures (CapEx) of electrolysis—defined as the cost of the electrolyzer and ancillary equipment, along with installation costs and other fixed costs—would also need to meet an equivalent of $1/kg H2 while utilizing this low-cost electricity. This may be currently feasible with high capacity factors, but for pairing electrolysis with renewable energy sources that provide low-cost electricity, capacity factors on the order of 30–40% are more realistic.2,134,
3.1.2. Renewable Energy Coupling
Increasing the capacity factor is the second most important cost factor, only behind electricity costs (Figure 4).136 However, to couple PEMWEs with renewable energy, periods of low renewable energy supply will be inevitable. The temptation, then, is to constantly have PEMWEs draw power from the grid, even during such periods. However, coordinating with the grid to provide energy during these times is not always possible and is generally prohibitively expensive. Furthermore, even if there is enough power locally, utilities prefer PEMWEs to draw power only during periods of excess renewable supply so as to not exasperate grid balancing issues. Thus, grid control algorithms and management strategies are required.
Figure 4.

Sensitivity analysis for the cost factors of hydrogen production. Adapted from ref (136). Copyright 2020 U.S. Department of Energy.
Since current PEMWEs are optimized for constant-load operation, load fluctuations from renewable energy coupling can accelerate the degradation of critical components, leading to lower system lifetimes. For example, anode catalyst layers are especially sensitive to such fluctuations and can be the limiting factor in stack lifetimes.137 BOP components (e.g., pumps, driers, hydrogen compressors) can also suffer from such operation. Since system lifetimes directly influence overall hydrogen costs, innovative strategies to provide more consistent power—such as utilizing energy storage, dynamic/intelligent controls, or multiple renewable energy sources—are necessary. An example of intelligent control can be demonstrated using a 600 MW plant (Figure 5) consisting of sixty 10 MW arrays (arrays contain multiple stacks): if the power input for a given period oscillates between 100 MW and 300 MW, instead of operating all 60 arrays at 17–50% power, one can operate 30 arrays at 33–100% power.
Figure 5.

600 MW PEMWE concept plant utilizing sixty 10 MW arrays (from Plug Power).
In summary, balancing renewable energy integration with potential economic repercussions—namely, low capacity factors and increased degradation—will be essential as PEMWEs scale up. However, given the limitations of electricity costs and renewable energy coupling, reductions in CapEx will be necessary to meet hydrogen cost targets.
3.1.3. Capital Expenditures
Given its
clean hydrogen cost targets ($2/kg by 2026 and $1/kg by 2031), the
US DOE carried out an analysis that indicates that PEMWE CapEx of
$300/kW by 2026 and $150/kW by 2031 (one kW can produce ∼0.5
kg H2 daily6) are required.138 Assuming a modest 50,000 hours of operation,
a PEMWE produces approximately 1000 kg H2/kW nameplate
capacity, and thus a CapEx of $150/kW would contribute $0.15/kg
to the hydrogen production cost. Further
studies indicate that even with such a CapEx reduction, the latter
target of $1/kg H2 is still out of reach due to operating
expenditures (OpEx; ongoing costs associated with operation, e.g.,
costs due to electricity, part replacements, routine maintenance,
labor, etc.) related to the price of electricity, even in regions
of the United States with high renewable electricity potential. Thus,
reductions in OpEx and further reductions in CapEx than those targeted
by the DOE are required.139 Opex reductions
can be achieved by lowering renewable electricity costs, developing
more efficient and/or durable PEMWEs, and operating in lower current
density regimes (although the last entails a trade-off with increasing
CapEx due to lower capacity factors, leading to variable optimal current
density regimes as a function of electricity costs).13
Current CapEx of PEMWEs is observed in a wide range of ∼$800–$1500/kW.140−144 Future CapEx has been estimated by several methods including literature surveys,131,145 industry surveys,146,147 learning curve estimates,144,148 and bottom-up cost analyses.142,149 Across the breadth of these studies, future CapEx is generally expected to hit the range of $200–$600/kW, with high variation largely due to differences in assumptions regarding 1) the rate of production scale-up, and 2) the impacts of economies of scale and learning rates on cost reduction.150Figure 6 shows several recent cost projections using a variety of techno-economic (TEA) methods, along with notable cost targets. Cost targets clearly hinge on optimistic CapEx reduction scenarios or lie outside of current projections. Considerable research and development are required to bridge this gap between CapEx projections and targets.
Figure 6.
PEMWE CapEx projections with confidence intervals shaded in (Horizon 2020,151 IEA,5 WEC,152 Bohm et al.,144 FCHJU,146 and Glenk et al.131), as well as CapEx targets for enabling economically competitive green hydrogen (FCHJU,153 U.S. DOE,154 and IRENA141).
3.1.4. Carbon Pricing
Before discussing methods to reduce CapEx, it should be noted that placing a price on carbon emissions for hydrogen production—either in the form of carbon taxes or a carbon market—can be a significant economic driver for green hydrogen. For PEMWEs to reach cost parity with SMR-based hydrogen production, a carbon tax of $230–$550/ton CO2e (“e” is global warming potential equivalent) is required. Blue hydrogen is expected to reach cost parity with gray hydrogen with a more modest $50–$60/ton CO2e.53 In addition, carbon markets have grown tremendously in recent years, with 24% of global emissions covered by either a national carbon tax or carbon market. Notable carbon markets include emissions trading systems (ETS) such as the European Union ETS and California’s Cap and Trade Program, which saw prices of $60/ton CO2e and $40/ton CO2e, respectively, in 2023.
3.2. CapEx Reduction
The primary driver to decreasing PEMWE CapEx over the next decade is increasing manufacturing capabilities in both unit size and production volume, with companies aiming for MW-scale unit sizes (compared to kW-scale) and GW/yr production volumes. In addition to improving equipment utilization and spreading fixed costs (such as labor) over a greater production volume, CapEx reductions require implementing more effective large-scale manufacturing processes, which include automation and roll-to-roll assembly.155
PEMWE systems consist of the stack and the balance of plant (BoP), which provides the fluids handling, thermal conditioning, power conditioning, and controls needed to facilitate the reactions occurring in each cell. According to a detailed TEA of CapEX as a function of production volume (Figure 7), a cost split of roughly 40% stack and 60% BoP is observed at lower volumes (approx. <20 MW),149 which is generally in-line with other analyses.134,141,142 As production rates scale-up (approx. >100 MW), BoP costs become increasingly dominant, comprising upward of 70% of the manufacturing cost. A third of the manufacturing cost can be attributed to power supplies alone, which is required to convert high voltage AC or DC electricity to the low voltage and high current DC electricity needed for electrolysis. AC/DC thyristor-type rectifiers are most commonly utilized due to their reliability, technological maturity, and comparatively low cost.156 The effect of economies of scale is presumed to be not as impactful on BoP components, which are largely outsourced. This was observed to be the case with BoP costs for PEM fuel cell (PEMFC) power plants as they scaled up, particularly with the AC/DC power conditioning equipment.157
Figure 7.
CapEx breakdown of a 1 MW PEMWE system by bottom-up manufacturing analysis projected out by production volume (a) and production volume and R&D-driven cost reductions (b). As a note, “Economies of Scale” encompasses manufacturing engineering in (b). Adapted from ref (149). Copyright 2019 National Energy Renewable Laboratory (NREL).
At the stack level, costs can be broken down into MEAs, PTLs, frames, BPPs, end plates, assembly labor, and balance of stack. Balance of stack refers to additional components such as wires, insulation, and compression hardware, and can make up around 13% of the stack cost.158 In order of contribution, MEAs are the most expensive component, followed by PTLs, BPPs, and then end plates and framing. At higher production volumes where labor costs are lower, material costs begin to dominate and MEAs can comprise nearly half of the stack cost due to the membrane material and expensive platinum-group metal (PGM) catalysts used. Furthermore, PTLs and BPPs are commonly made of titanium and currently require expensive coatings, typically gold or platinum.
In order to reach the U.S. DOE CapEx target of $150/kW by 2031, stack costs need to be brought down significantly from current values of $237/kW. Several pathways have been identified to reduce stack costs, primarily focused on reducing material costs, increasing stack efficiency, and achieving higher current densities.159 Although current densities as high as 15 A·cm–2 have been observed,160 attaining greater current densities alone is not sufficient to reduce costs as such high current operation is only beneficial when low-cost electricity is available.161,162 Thus, focus also needs to be put on reducing material costs and improving stack efficiency, both of which will require the optimization of individual cell components.
4. Component Improvements
This section will examine all the primary components in a PEMWE cell and establish research levers for GW-scale deployment. Challenges in fundamental research, cost, and manufacturability will be thoroughly discussed.
4.1. Anode Catalyst Layer
A conventional anode catalyst layer (CL) consists of a catalyst dispersed in an ionomer (an ionically conductive polymer) network coated on either a membrane—in the case of a catalyst-coated membrane (CCM)—or a PTL—in the case of porous transport electrode (PTE). Additionally, “membrane–electrode assembly” (MEA) is a general term that refers to the membrane and adjacent CLs, with no distinction between CCM and PTE configurations. Multiple methods to coat a CL onto a substrate (e.g., a membrane or PTL) can be employed, such as airbrushing, ultrasonic spraying, or doctor blade coating.163 The MEA configuration and CL coating method can influence CL properties and cell performance; such impacts have been thoroughly reviewed by Wang et al.163 Thus, this section will focus on smaller-scale considerations, such as loading reductions, catalyst utilization, catalyst supports, and CL microstructure.
The catalyst must be stable under the highly acidic (pH ∼ 0; due to the presence of protons from the OER) and oxidizing (>1.3 V) conditions of the anode, which currently limits the material selection to precious metals.164 While ruthenium is one of the most active OER catalysts, its lack of stability has resulted in iridium being the primary choice.8 Iridium oxide (IrOx) is the most commonly used form of iridium catalysts since metallic iridium is less active.165,166 Activity and durability are highly dependent on the surface state of the iridium, with amorphous IrOx showing higher activity and lower durability than crystalline IrOx.167 Mom et al.167 attributed these properties of amorphous IrOx to greater deprotonation depths under OER potentials. However, the catalyst can undergo chemical changes when experiencing varying cell potentials or being in contact with hydrogen (from cathode crossover). Rheinlander et al.168 reported that crystalline IrO2 can be transformed into amorphous IrOx or even metallic Ir, based on operating conditions. Thus, changes in the catalyst state should be meticulously monitored, especially during long-term testing.
Minimizing the amount of iridium used in anode CLs is vital for reaching cost targets. Between the use of platinum in the cathode and iridium in the anode, iridium is the bottleneck in scale-up due to its rarity (7.5 tons of iridium is mined per year, compared to ∼200 tons for platinum169).170 In the literature, notable progress has been made to reduce loadings from >1 mgIr·cm–2 to below 0.5 mgIr·cm–2.166,172−177 However, further efforts must be made to enable large-scale fabrication of these low-loading CLs, such as 1) obtaining a fundamental understanding of interfacial transport mechanisms, 2) identifying degradation modes, and 3) ensuring quality control at greater production volumes.163 Understanding transport mechanisms by unveiling the interplay between electrons, protons, water, and oxygen in low-loading CLs is required to achieve comparable performance with high-loading CLs. Moreover, identifying degradation modes will enable us to tune CL structure for improved durability. Lastly, translating laboratory-scale fabrication methods to large-scale production for low-loading CLs is of utmost importance for scale-up but has largely been overlooked in the field.
4.1.1. Catalyst Utilization
Optimizing transport processes in/around the CL (illustrated in Figure 8) is a prerequisite for high catalyst utilization at low loadings. To sustain the OER, the CL must facilitate the transport of protons, electrons, liquid water, and gaseous oxygen. Protons move through the ionomer phase in the CL to the membrane. Electrons move through iridium particles in the CL to the particles in the PTL. Notably, isolated iridium particles and iridium particles that are fully embedded in the ionomer phase will likely not conduct electrons as ionomers are electronically insulating. Lastly, the PTL allows liquid water to permeate through its pores (in the scale of tens of μm)178 to the pores in the CL (in the scale of nm)179 while simultaneously facilitating oxygen gas removal.
Figure 8.

Transport processes occurring in/around the anode catalyst layer (CL). Reactant liquid water permeates through PTL pores to CL pores. Product gases flow in the counter direction from CL reaction sites to PTL pores. Proton transport occurs through the CL ionomer phase and the membrane, while electronic transport occurs through the iridium particles in the CL and PTL particles in the PTL.
The interface where PTL, catalyst, and ionomer meet—termed the “triple-phase boundary”—plays a vital role in catalyst utilization as the OER can only occur here. Notably, iridium particles that do not directly contact the PTL can still participate in the OER if they are electronically connected to the PTL through other iridium particles. At low iridium loadings, such a connected network is less likely to exist. Thus, particles not directly contacting the PTL are less likely to be utilized, reducing the triple-phase boundary. Consequently, when CLs swell (simply due to water uptake from the ionomer) into the void space of the PTL—a process known as delamination—the iridium particles in the CL spread apart and become more disconnected, leading to lower electronic conduction and, hence, lower catalyst utilization.180 Poor catalyst utilization resulting from delamination is particularly severe at low loadings due to the low density of iridium particles.
While low iridium-loading MEAs have shown high performance in some cases,163 strategies to alleviate issues of electronically insulated—and thus unutilized—iridium particles will likely be required. Due to the dependence of catalyst utilization on both the CL and PTL, strategies to improve utilization regarding the PTL will be discussed in Section 4.4.4. However, strategies regarding the CL also exist. The first is proposed by Hegge et al.,181 where isolated iridium particles were bridged together by depositing a layer of iridium fibers (fabricated via electrospinning) on top of them. The second is by Chatterjee et al.,182 where utilization was enhanced by completely changing the catalyst morphology: instead of iridium nanoparticles (which are typically used for CLs), the authors synthesized nanoporous iridium nanosheets (via electrochemical dealloying of nickel–iridium foils) that provide a continuous, connected structure. However, these two strategies are relatively new; a more widely studied strategy to increase utilization is to use catalyst supports.
4.1.2. Catalyst Supports
In principle, dispersing a catalyst on a support should increase its surface area-to-mass ratio, thereby reducing the catalyst mass needed to achieve a desired current. Hence, supports hold significant potential for loading reductions. As detailed below, the critical challenge is that the most commercially available support, TiO2, is electronically insulating; thus, the benefit of increased catalyst dispersion is partially countered by electronically isolating the catalyst. Many research efforts have long sought to develop conductive support materials, either by doping TiO2 or finding new materials entirely, but none have achieved successful long-term durability testing as TiO2 has. If TiO2 is used, the iridium oxide must act as the electron conduit (not the TiO2). Therefore, connected pathways of iridium oxide on the catalyst support and within the CL are needed to ensure iridium utilization.
4.1.2.1. Material Selection
For supports to be viable, the material must be stable in the operating conditions. The highly acidic and oxidizing conditions of the anode render most support materials—conductive carbon black included—thermodynamically unstable.183 Most of the remaining (more) stable materials are semiconducting metal oxides, which present inherent conductivity concerns. Nonetheless, several novel catalyst supports have demonstrated promising performance in rotating disk electrode and/or MEA setups, including TaC,184,185 Sb2O5–SbO2 (ATO),186−188 NbC,185 TiC,185 WC,185 NbO2,185 and W2B.189 Their accomplishments notwithstanding, this review will not cover these supports given the scarce literature with low loadings and durability testing at industrially relevant current densities (>1 A·cm–2). We refer the reader to a review on emerging supports,190 and we look forward to more progress in these novel materials.
TiO2 as a support has increasingly been tested at industrially relevant current densities with low iridium loadings and thus will be the focus of this section. The interest in TiO2 as a support for the OER can be traced back to the commercial implementation of RuO2 on TiO2 via dimensionally stable anodes (DSAs) for the chlorine evolution reaction, which has an even higher redox potential than the OER (1.36 V vs 1.23 V).191 This technology established the relevance of metal oxides as anode catalysts and supports. There are primarily two commercial IrOx/TiO2 (i.e., IrOx supported on TiO2) catalysts in recent literature: Umicore Elyst Ir75 (IrO2/TiO2, diameter ∼28 nm)168,192−197 and Heraeus P2X (IrOOHx/TiO2, diameter ∼284 nm).194,195,197
4.1.2.2. Conductivity Issues
Despite its high stability, TiO2 supports come with the caveat of high electronic resistivity. While a common catalyst support for PEMFCs, Vulcan-XC72, has a resistivity of ∼0.4 Ω·m, values for TiO2 (in nanowire form) are upward of 4000 Ω·m.198 Several studies have attempted to bypass this issue by using more reduced forms of titanium. At low loadings (<0.3 mgIr·cm–2), IrO2/Ti has been shown to increase electrochemically active surface area (ECSA) and overall outperform unsupported IrO2.199 Others have studied Magneli phase titanium oxides (i.e., substoichiometric oxides of the form TinO2n-1), finding increased electronic conductivity relative to TiO2200 and enhanced performance relative to unsupported catalysts.201 However, whether these supports remained in their reduced state throughout operation was left unaddressed.
Since IrOx films and single crystals have resistivity values many orders of magnitude lower than TiO2 (∼10–8 Ω·m),202,203 it is believed that the deposited IrOx on titanium supports provides the electronic conductivity within the CL. In principle, if a true core–shell structure is achieved, there will be complete conductivity and IrOx utilization. In practice, however, complete films of IrOx on TiO2 are difficult to prepare; hence, electronically isolated islands of IrOx on TiO2 often result. Thus, to achieve high electronic conductivity within the CL, interconnected networks of IrOx long enough to reach catalyst particles not in direct PTL contact would be required. This type of network would reduce the probability of electronically disconnected catalyst particles and thereby increase catalyst utilization.
4.1.2.3. Electronically Conductive Networks
Two strategies have been employed to help enable electronically conductive networks: optimizing CL thickness and developing core–shell catalyst structures.
CL thickness is a metric correlated with catalyst utilization, as a CL that is too thin will have less interconnected iridium particles and thus a lower probability of forming a complete in-plane (i.e., parallel to the membrane) electronic conduction network throughout the CL. Hence, it is necessary to maintain a certain CL thickness to avoid such issues. Through cross-sectional SEM, the thickness of the CL is shown to be linearly proportional to iridium loading.193 Through experiments using Umicore Elyst Ir75 (IrO2/TiO2) with various Ir loadings between 1–2 mgIr·cm–2, Bernt et al.193 proposed an optimal anode CL thickness of 4–8 μm. The lower bound (4 μm) ensures adequate in-plane electronic conductivity, while the upper bound (8 μm) limits mass transport overpotentials, as thicker CLs suffer from water transport issues. In a later study,194 Bernt et al. calculated that a low packing density Heraeus P2X would require a loading of 0.06 mgIr·cm–2 to form a 4–8 μm thick CL, as opposed to the 0.56 mgIr·cm–2 required for Umicore Elyst Ir75. While the logic of using larger support particles to enhance CL thickness (without increasing iridium loading) is sound, increased CL thickness does not necessarily equal increased CL conductivity if percolating IrOx networks are not present.
Several studies have sought core–shell structures where percolating IrOx networks would provide the needed electronic conductivity at low loadings.197,205−1000 De Angelis et al.207 demonstrated connected films of IrO2 supported on TiO2 in a CL via X-ray ptychographic tomography (a nondestructive 3D imaging technique), although the loading was very high—3 mgIr·cm–2. Given the well-connected pathways for IrO2, the authors concluded that “for any CL where the percolation of the IrO2 is ensured, any high-surface area support material can be employed, even if fully electrically insulating.” The concept has been extended to PTE configurations as well, with one study featuring an IrO2/TiO2 core–shell catalyst (0.4 mgIr·cm–2) that performed better than the Umicore IrO2/TiO2 catalyst (0.5 mgIr·cm–2).208 While increased electronic conductivity is beneficial, it is possible that CL conductivity is not as critical for PTEs as for CCMs, given that the catalyst in PTEs is directly deposited on the PTL.
In summary, using TiO2 as a support is not a guarantee of increased catalyst utilization as the insulating nature of TiO2 can render IrOx particles electronically isolated (and therefore unutilized) unless there is a percolating network of IrOx domains. That said, there have been demonstrations of promising performance at loadings below 0.4 mgIr·cm–2, even after thousands of hours of testing.195,199 Further investigations in creating percolating IrOx pathways under low loadings are warranted. Lastly, alternative materials and doped TiO2 are showing promise and should be examined for long-term durability, as finding a conductive support (that is stable) would eliminate this percolation challenge.
4.1.3. Durability
While researchers seek to lower catalyst loadings to meet cost targets, care must be taken to ensure that durability is not compromised during the process. However, as reviewed by Wang et al.,163 only six MEA studies have examined iridium durability at loadings ≤0.4 mgIr·cm–2. Hence, mechanisms of degradation and parameters that exacerbate degradation still need to be clearly identified for low-loading systems.
To understand IrOx degradation mechanisms, Yu et al.173 conducted a microscopic analysis of an ultra-low-loading CCM (0.08 mgIr·cm–2) under industrially relevant conditions (1.8 A·cm–2, ∼30 bar pressure, 86 cm2 active area). They found that 70% of the initial iridium was lost after 4500 hours of operation. Numerous other studies have also found significant iridium dissolution over time, with the membrane and cathode CL being the primary sinks for subsequent redeposition.137,211−214
Parameters shown to be highly degrading to the anode CL are open-circuit voltage (OCV; relevant during startup/shutdown operation) conditions, dynamic operation, and low iridium loadings. Weiß et al.212 investigated the impact of a 1.3 V hold versus an OCV hold in a cycling profile. Two protocols were used (as depicted in Figure 9a): An OCV test (3 A·cm–2, 0.1 A·cm–2, and OCV steps) and a reference test (3 A, 0.1 A, and 1.3 V steps). The former resulted in more degradation due to the OCV conditions reducing the crystalline IrO2 (the starting material) to metallic Ir and then oxidizing it to amorphous IrOx (which is less stable). Overall, they found a very high degradation rate of ∼300 μV/h for this test and, surprisingly, a negative degradation rate (i.e., performance increased over time) for the reference test (both used a high loading of 1.75 mgIr·cm–2). Incorporating the OCV hold instead of the 1.3 V hold led to faster iridium dissolution and increased HFR (due to the crystalline IrO2 transforming into a less conductive hydrous iridium oxide).
Figure 9.
(a) Current density and voltage profiles (of one cycle) for the OCV test and reference test used to examine the impact of OCV holds on cell performance. Adapted from ref (137). Copyright 2019 The Authors under Creative Commons Attribution Non-Commercial No Derivatives 4.0 License (http://creativecommons.org/licenses/by-nc-nd/4.0/). (b) Polarization curves after 525 hours of operation with square wave cycling protocols from 1.45 V to various upper potentials ranging from 1.6 V to 2.5 V. Initial (i.e., beginning of life) polarization curve is shown in orange. Adapted from ref (212). Copyright 2019 The Authors under Creative Commons Attribution 4.0 License (http://creativecommons.org/licenses/by/4.0/).
Regarding dynamic operation and loadings, Alia et al.137 examined durability at low loadings (0.1–0.4 mgIr·cm–2) and reported that potential cycling resulted in greater degradation than potential holds. Furthermore, square wave cycling was more damaging than triangle wave cycling, suggesting that sharper transitions accelerate degradation. They also found that greater cycling frequencies and higher upper potentials (Figure 9b) accelerate degradation. Moreover, the impact of catalyst loading on durability was also investigated. While they observed minimal degradation at 0.4 mgIr·cm–2, meaningful degradation was found at 0.1 mgIr·cm–2. The authors hypothesized that degradation is not inherently loading-dependent, but rather, the extra thickness of the CL at higher loadings acts as a buffer that delays the onset of degradation. A 1000 hour low-loading MEA stability test by Rozain et al.199 backs up this hypothesis, as they found that two CLs with a similar thickness but a different loading (IrO2/Ti at 0.1 mgIr·cm–2 and pure IrO2 at 0.32 mgIr·cm–2; the same IrO2 was used) had comparable durability.
Standardized accelerated protocols to characterize degradation will need to be developed to test durability more quickly (i.e., without having to operate cells over thousands of hours). Furthermore, standardization will allow the community to objectively compare MEAs with different loadings and morphologies. For instance, different fabrication methods (e.g., blade coating vs spray coating) result in distinct CL morphologies, and the nature of their degradation can differ significantly.163 Thus, universal protocols are a prerequisite for efficient research in developing next-generation MEAs. Recommendations for such protocols will be discussed in Section 5.1.
4.1.4. Ionomer Binders
As mentioned previously, CLs typically consist of catalyst particles dispersed in an ionomer network. The CL must expose the surface of catalyst particles for reactions, maintain proton and electron conducting pathways, enable reactant transport to catalyst sites, and remove reaction products—all of which are impacted by the ionomer. Please note that since ionomers are used for both the membrane and CL, “ionomer binders” will refer to CL ionomers only. In commercial MEAs, the ionomer binder has an identical or similar chemical composition to that of membrane ionomers. Some ionomer properties (such as ionic conductivity) are beneficially optimized in the same direction for membranes and binders. Other properties that are essential to membrane applications prove detrimental to binder applications, including high electronic resistance and low gas permeability. As there does not exist a single material ideal for both applications, a similar (often identical) ionomer to the membrane is employed as a binder to enable proton conduction within the CL, which has a strong impact on the overall optimization of CL proton conductivity, electronic conductivity, and mass transport.
The GW-scale deployment of CLs in PEMWEs can leverage decades of fundamental understandings of catalyst/ionomer integration from PEMFC research. For example, Raistrick217 demonstrated that by replacing PTFE with an ionomer binder, platinum utilization was improved to the point where loadings could be reduced by an order of magnitude (leading to their ubiquitous inclusion in PEM devices). Baker et al.218 and Greszler et al.219 identified an unknown transport resistance in PEMFC cathodes associated with the ionomer, which was later demonstrated to arise from a local oxygen transport resistance due to the ionomer orientation at the platinum–ionomer interface.220,221 The findings from these studies suggest the importance of considering a holistic set of properties for binder candidates and how they impact transport properties in PEMWE CLs, especially as iridium loadings are driven lower.
While much can be learned from PEMFC research efforts, novel PEMWE configurations are also being explored that have the potential to influence ionomer selection and where it is deployed. Where most PEMWEs feed liquid water to the anode directly, some systems rely on water vapor-fed anodes or back-diffusion from liquid water-fed cathodes,222,223 which could influence the optimal anode CL composition in unexpected ways. Furthermore, Lee et al.224 demonstrated a promising strategy whereby a low loading of IrOx was deposited directly onto the PTL, avoiding the need for ionomer binders entirely. Overall, the role of the ionomer in scalable, durable, and high-performing CLs in PEMWEs will require further investigation to enable deployment at scale.
4.1.5. MEA Fabrication
Finally, large-scale production methods for low-loading CLs requires more development. The majority of the low-loading MEAs tested in the literature uses ultrasonic spray coating, which requires a catalyst ink with relatively low solid ratios (<1 wt %).175,177,181,225−227 However, this technique is not suitable for large-scale production due to its low throughput.226 Blade coating techniques (e.g., doctor blade coating, rod coating, slot die coating), on the other hand, are more scalable but require inks with higher solid ratios (>5 wt %),227 which tend to result in inhomogeneous CLs when lower loadings are targeted. Thus, more research is required to enable large-scale fabrication of low-loading MEAs, likely via blade coating techniques. Two research levers include 1) understanding the key parameters of catalyst inks that will allow for uniform CLs and 2) minimizing catalyst loss from ink intrusion into PTL pores during PTE fabrication. More examination in topics such as these will be essential for curtailing PGM usage.
4.2. Cathode Catalyst Layer
Platinum black supported on carbon (Pt/C) is the standard cathode catalyst for PEMWEs. Studies on Pt-free catalysts have been reviewed228,229 but remain an active research area. Given the sparsity of durability studies with such catalysts, this section will be limited to Pt-based catalysts.
Although studies utilizing Pt-based cathode catalysts typically assume negligible cathode contributions to cell overpotential, the true contribution may not be obvious, especially when considering OCV conditions. On the one hand, one model estimated cathode overpotentials (for a single cell) of less than 1 mV at 3 A·cm–2230 and one experimental study found that performance was insignificantly affected by Pt loading reductions from 0.30 mgPt·cm–2 to 0.025 mgPt·cm–2.193 However, a modeling study of a 12-cell, 5.6 kW stack found that cathode overpotentials can reach up to 63% of the anode overpotential when the cathode pressure is increased to 70 bar.231
4.2.1. Overpotentials
Cathode overpotentials were not experimentally verified in (single-cell) PEMWEs until the introduction of in situ reference electrodes, which were recently reviewed.232 In one study with such an electrode (3 mg·cm–2 Pt black for the cathode, 3 mg·cm–2 Ir0.7Ru0.3O4 for the anode), when the load was switched from 1 A·cm–2 to open circuit potential (OCP) conditions, the cathode potential evolved from −0.06→1.05 V vs. RHE and the anode potential from 2.00→1.25 V vs. RHE.233 While these measurements confirm that the anode overpotential (∼0.77 V) was over a magnitude larger than that of the cathode (∼0.06 V), it also showed that the cathode experienced a more significant change in half-cell potential during the transition from operation to OCP, which was attributed to Pt oxidation due to crossover oxygen (from the anode). A later study tracked the evolution of the cathode overpotential alongside in situ Pt dissolution measurements via a hanging mercury drop electrode.234 The resulting heat map of Pt dissolution—as a function of load (at 1 A·cm–2) and OCP duration—found the most degrading condition to be cycling between 1 A·cm–2 for 0.01 h and OCP for 7.9 h. Notwithstanding, a 1000 h study utilizing a five-cell stack found that a constant 2 A·cm–2 hold resulted in increased overall cell degradation compared to alternating between OCP and 2 A·cm–2 (for both 10 min and 6 h at each condition).235 These two studies are not necessarily in disagreement; even if Pt dissolution—and perhaps cathode degradation—is highest when alternating between operation and OCP, the overall cell degradation was still more pronounced during operation, agreeing with the consensus that the anode defines the majority of degradation.
The only known AST study utilizing an in situ reference electrode236 examined the evolution of half-cell potentials over 1000 hours while employing a dynamic load degradation test (defined by the EU Harmonized Protocols for Testing of Low Temperature Water Electrolysers). While the anode experienced a substantial increase in half-cell potential during the first week and the cathode did not, the rates of half-cell potential increases were similar for both in the subsequent weeks. However, the authors noted that half-cell potential measurements were sensitive to even slight movements of the reference electrode, with many results potentially explained by either a physical change or a disturbance of the reference electrode. Unfortunately, these events are especially relevant when working with long-duration tests, where unanticipated shutdowns and adjustments are common.
4.2.2. Post-Mortem Analyses
Given the challenges of long-duration in situ half-cell monitoring, post-mortem analyses become especially relevant to understanding cathode degradation, although studies are sparse. A previously mentioned study (in Section 4.1.3) by Yu et al.173 examined low-loading (0.3 mgPt·cm–2; 0.08 mgIr·cm–2) CCM degradation (4500 h of operation at 1.8 A·cm–2) with cross-sectional SEM coupled with EDS (SEM/EDS). Pt/Ir bimetallic particles were observed in the membrane (on the side closer to the cathode), and Ir particles were observed in and adjacent to the cathode CL. Although Ir degradation was the most pronounced—with 70% of the original Ir lost—Pt degradation was not negligible, with 10% of the original Pt lost (to the membrane), which was understood to be due to the transient reduction of Pt oxides at the beginning of the test. A similar study using cross-sectional SEM/EDS has also observed Pt and Ir particles in the membrane after 4000 hours of startup/shutdown cycling.237 Lastly, Rakousky et al.238 used post-mortem TEM imaging after 1000 hours of operation (at 2 A·cm–2) and observed that the average Pt particle size increased from 3.5 nm to 7.8 nm. However, the authors concluded that it was unlikely that this particle growth significantly contributed to decreased cell performance, instead citing PTL corrosion and anode activity reduction.
4.2.3. Outlook
In conclusion, the assumption that cathode overpotentials negligibly contribute to beginning of life single-cell performance is supported by experimental results, but it is unclear whether this holds true for multi-cell stacks (especially at higher pressures). In situ monitoring of half-cell potentials becomes especially challenging for extended studies due to unexpected adjustments/changes to the reference electrode. The studies presented suggest that cathode contributions to degradation are strongly masked by those of the anode for single-cell durability. Future single-cell durability studies could benefit from in situ reference electrodes, although precautions must be made to ensure a stable reference electrode. Post-mortem studies can contribute substantially to understanding degradation processes, but there are still gaps in linking Pt degradation to PEMWE performance loss; such gaps could be addressed with modeling studies. Additionally, future studies utilizing multi-cell stacks and higher pressures could benefit from elucidating these effects as well. Such studies would benefit from the collaboration between academic institutions and industrial companies, with the former spearheading electrochemical/post-mortem studies while the latter provides the necessary equipment for such experiments.
4.3. Membrane
The type of membrane used in PEMWEs is a proton exchange membrane (PEM) and is responsible for conducting protons and preventing gas crossover. While the membrane neither contributes significantly to costs nor is a substantial factor for cost reductions through economies of scale (Figure 7b), membrane research is a primary lever for voltage efficiency and lifetime improvements.
State-of-the-art membranes are based on perfluorosulfonic acid (PFSA) chemistry. PFSA is a copolymer of tetrafluoroethylene (used in Teflon) and a sulfonic acid-terminated perfluorinated monomer (Figure 10a). This combination of a hydrophobic backbone and hydrophilic side chain results in a phase-segregated structure in which cation-conducting water channels form and percolate through a solid matrix. Distinctions between PFSA membranes and hydrocarbon alternatives (Figure 10b) will be discussed in Section 4.3.5. For many decades, PFSA membranes have enabled PEMWEs to 1) operate at high current densities, 2) operate under dynamic electrical loads, 3) achieve high energy efficiencies, 4) produce high purity hydrogen (up to 99.999%), and 5) achieve long lifetimes.239
Figure 10.

Prototypical structures of two proton exchange membrane (PEM) chemistries. (a) PFSA-based: a hydrophobic tetrafluoroethylene backbone with a hydrophilic side chain ending with a sulfonic acid group. (b) Hydrocarbon-based: a network of rigid hydrophobic aromatic groups with sulfonic acid groups attached at some ends.
4.3.1. Targets
Membrane-related targets set forth by the U.S. DOE are shown in Table 2.240 State-of-the-art membranes (such as Nafion N115) have excellent durability (leading to high lifetimes) but elevated ohmic overpotentials due to their high resistance to proton transport. Reducing this inefficiency will likely involve some combination of a more conductive ionomer and a reduced membrane thickness. However, these changes can impose mechanical strength and gas crossover challenges, especially when operating at high differential pressures (≥30 bar).241 Insights in improving performance in these areas will be summarized, along with perspectives on developing a composite membrane enabling 2026 (and beyond) U.S. DOE targets.
Table 2. Membrane-Related Targets for PEMWEs (80°C, 30 bar Differential Pressure)240,242.
| parameter | units | current status (Nafion N115) | 2026 target |
|---|---|---|---|
| Lifetime | h | 60,000 | 80,000 |
| Degradation Rate | %/1000 h | 25 | 13 |
| Activity @ 3 A·cm–2 | V | 2.0 | 1.8 |
| PEM Thickness | μm | 125 | 50 |
| PEM Resistance | mΩ·cm–2 | 100 | 30 |
| H2 Crossover | % H2 in O2 | 2 | 0.5 |
4.3.2. Ohmic Losses
Improving voltage efficiency is largely incumbent on reducing membrane proton transport resistance. For a given operating condition (e.g., temperature), two factors can reduce this resistance: 1) improving ionomer conductivity and 2) minimizing membrane thickness.
The conductivity of a PFSA ionomer is a strong function of its equivalent weight (EW), defined as the mass of polymer per mole of sulfonic acid (g/mol). In an ionomer review,243 conductivity as a function of EW for many ionomers was evaluated, and it was shown that many ionomers have a lower EW than that of N115 (1000 EW). However, a strong lower bound for EW exists for practical applications dictated by a given ionomer’s water uptake/solubility. As water uptake increases from decreased EW, issues such as low mechanical strength and high gas crossover can arise that may counteract the benefit of proton conductivity increases. Furthermore, the differences in ionomer conductivity from different EWs are minimized in the liquid-saturated PEMWE environment.244
Apart from a significant ionomeric breakthrough, much of the reductions in resistance will likely come from thinner constructions. As early as 2015, Lewinski et al.245 reported a 50 μm membrane achieving 1.77 V at 3 A·cm–2 (80 °C), which is ∼150–200 mV lower than for standard N115 membranes. Furthermore, Garbe et al.246 observed a ∼240 mV decrease at 3.0 A·cm–2 when comparing a 183 μm and 50 μm membrane. However, making membranes thinner makes them more susceptible to mechanical deformation and gas crossover. Utilizing reinforcements can potentially alleviate these issues.
Membrane reinforcements have been used in more mature electrochemical devices (e.g., chlor-alkali and hydrogen fuel cells) for 1) improved mechanical durability (by giving resistance to crack formation and through-plane defect penetration), 2) lower expansion in water and other solvents, and 3) processability during manufacturing and cell assembly. For PEMWEs, an early example of a reinforced membrane is the directionally stable membrane (DSM) developed at Giner, where holes were formed in a flat reinforcing material. While significant morphology optimization occurred, it is unclear whether an economical route to manufacturing DSMs at scale was ever realized.247 More recent examples include woven fabrics and cloths (based on fluorocarbon or hydrocarbon fibers)248 and nonwoven meshes (such as expanded polytetrafluoroethylene (ePTFE) or electrospun materials).249,250 The ideal reinforcement is one that provides increased durability and reduced crossover and can be manufactured at a low cost and high volume.
4.3.3. Gas Crossover
Hydrogen gas crossover from the cathode to anode can lead to the formation of explosive mixtures as the lower explosive limit (LEL) of hydrogen in oxygen is just 4% (by volume). Thus, the greater crossover rate for thinner membranes is a major issue,251 especially when hydrogen is compressed in situ. This issue is exacerbated during periods of low electrical load (i.e., low current densities), where oxygen content is minimal.42 Three main strategies can be employed to mitigate gas crossover: 1) improving membrane gas-barrier properties, 2) implementing a recombination catalyst to react crossover hydrogen with oxygen (which forms water), and 3) utilizing BoP solutions such as pressurizing the anode stream or installing external air circulators to dilute crossover hydrogen. The membrane-based strategies (1 and 2) will be discussed herein; for strategy 3, we refer the reader to a review by Stähler et al.252
For gas barrier properties of a membrane, a common metric is the selectivity of proton (H+) transport versus molecular hydrogen (H2) transport (i.e., gas crossover). Not only does a higher selectivity reduce crossover, but it also increases the Faradaic efficiency of the cell (due to less cathodic H2 being lost from crossover).253 Several studies have explored the nature of H+/H2 transport in ionomers.254 Two studies by Stolten et al.255,256 demonstrated that H2 crossover through the membrane is purely diffusive. Fumagalli et al.257 studied PFSA ionomeric d-spacing as a function of time and revealed that the size of water channels never reach steady state, suggesting that membrane crossover could increase over time. Future ionomer design could incorporate these learnings to enhance selectivity. One strategy to improve selectivity (besides using reinforcements) is to incorporate nonionomeric fillers, such as graphene or graphene oxide, which are proposed to block gas crossover while enhancing H+ transport.258,259
In addition to improving gas-barrier properties, strategies to mitigate existing crossover H2 (i.e., H2 already present in the anode) will likely be necessary, as some level of crossover will always occur. Several strategies include a downstream H2 gas recombiner,260 a third electrode in the membrane,261 and a recombination catalyst (RC). All three strategies combine crossover H2 and O2 to form water, but RCs are the most commonly studied. They can be implemented in several locations, including as a coating on the PTL42 or anode CL,252 or within the anode CL262 or membrane.263 Furthermore, RCs can expand the operating current range in which PEMWEs can safely operate.264
RCs within membranes have been used for decades (first to increase humidity in PEMFC membranes38,265,266) and have several advantages, including 1) isolating the RC from high anodic potentials and 2) mitigating both H2 and O2 crossover (which minimizes peroxide formation at the CLs).252,267 RCs are typically PGM-based and can be implemented in membranes via 1) reduction of PGM salts to form RC nanoparticles in situ268 or 2) direct incorporation of preformed RC particles.27 The optimization of the RC location (within the membrane) and loading are active areas of study. For example, Gubler et al.269 studied three RC distributions in the membrane and found the most effective crossover mitigation occurred when the RCs were uniformly distributed. While research on RC optimization is progressing, insights into the long-term effectiveness of RCs over system lifetimes are lacking. Furthermore, the cost and complexity (i.e., the number of unit operations) for manufacturing RC-incorporated membranes must be minimized for facile uptake in future PEMWE systems.
4.3.4. Durability
Membrane durability should be one of the most prioritized research efforts, especially as designs tend toward thinner membranes for efficiency improvements. As early as 1988, PFSA membranes have enabled PEMWE durability above 10,000 hours.270 In 2006, a paper reported lifetimes of PFSA-based devices above 50,000 hours at moderate temperatures (∼50–60 °C).271 These findings illustrate that PFSA membranes have long enabled incredible durability—devices manufactured almost two decades ago have lifetimes that nearly reach 2026 targets. However, the significant reoptimization of membrane construction necessary to meet performance targets (i.e., incorporating reinforcements, RCs, more conductive ionomers, and thinner membranes) will represent a significant challenge to reaching future durability targets.
Fortunately, there have been several recent reviews covering membrane durability in PEMWEs.48,272−275 A high-level summary of their findings and perspectives on the most promising research efforts will be provided here. Membrane failure modes can be mechanical or chemical/electrochemical in nature. Membrane creep is a mechanical failure mode associated with membrane swelling and creep into the PTL/gasketing (for a visual of how membrane and PTL interact, refer to Figure 8). Other mechanical failure modes—such as pinhole formation and membrane dry-out—may arise from stack-level defects (e.g., inconsistent heating or water distribution, poor stack assembly). Chemical/electrochemical failure modes can also exist, including cation contamination and radical-induced degradation. Furthermore, multiple modes can be present simultaneously and could combine to accelerate degradation.276 Lastly, while not a failure mode itself, higher temperatures (which are used to reduce kinetic overpotentials and transport resistances) can accelerate the rate of each of these modes.271,276−278
4.3.4.1. Membrane Creep
Membrane creep can occur in both active (participating in electrochemistry) and inactive (gasketed) areas of the cell, along with the interface between the two. Creep failures have been identified as a limiting factor in cell lifetimes for thin membranes. For example, a study from Nel Hydrogen279 reported a ∼500 hour lifetime for a thin (89 μm) membrane compared to a ∼4500 hour lifetime for a thick (178 μm) membrane (both membranes were nonreinforced), where the lifetime gap was ascribed to membrane creep. Reinforcements have been identified as a solution for creep, as the same study also reported that a 60 μm reinforced membrane exhibited similar durability to the 178 μm nonreinforced membrane.279 However, there is a lack of mechanistic understanding of this failure mode as well as methods to evaluate its potential impact. The successful deployment of thin membranes will depend on understanding and quantifying membrane creep. Work tying fundamental mechanical properties to observed membrane creep will be critical toward mitigating these issues. Since creep might occur in a tensile mode (i.e., penetration into PTLs) and compression mode (as a result of compression under gaskets), multiple testing protocols might be required to evaluate creep in different cell areas.178,280
4.3.4.2. Cation Contamination
Cation contamination leads to reduced proton conductivity and increased overpotentials. Even with a pristine proton-form membrane at the beginning of life, several sources of contamination are conceivable, including feedwater impurities and dissolution of metal cell components (e.g., PTLs and BPPs).281 In principle, a small amount of infrequent cation contamination could be reversible, as the in situ generation of protons and excess circulation of liquid water provides a pathway for metal salts to exit the cell.282 However, flowing a preponderance of metal ions into the ionomer material could render the stack highly inefficient or inoperable (which is possible, for example, through an acute upset of water quality). Theoretically, the ionomer’s native protonic form could be refreshed by circulating an external acid solution.283 The practicality of this approach at GW-scales is unclear, and it could potentially extract beneficial additives such as RCs or radical scavengers (discussed in the next paragraph). The most cost-effective strategy to remediate ion contamination is to prevent it in the first place, as is often employed in water recirculation loops with a combination of reverse osmosis and ion exchange resins.275
4.3.4.3. Radical-Induced Degradation
The crossover of H2 into the anode or O2 into the cathode can lead to the formation of H2O2, which acts as the basis for radical species generation.284 Certain metals—such as Fe, Ti, Cr, Ni, Cu, Pt, and Ir—can catalyze H2O2 into harmful radicals such as H•, HO•, and HOO•.5,37,48,284 The reaction of these species have been documented as a central degradation mechanism in PEMWEs (and PEMFCs),285 but significant effort is still required to understand the fundamental nature of such degradation. Possible reactions of these radicals with PFSA ionomers are depicted in Figure 11. It should also be noted that changing the chemistry of a PFSA ionomer (such as adding bis-sulfonimide groups in the side chain) can potentially cause low stability against these radical attacks.286
Figure 11.

Possible radical-induced degradation mechanisms for PFSA ionomers. Sources: HO• attack on −COOH,287,288 HO• attack on ether linkages,289 HO• attack on −SO3H,289,290 and H• attack on C–F.291,292
To quantify radical-induced degradation, measurements of fluoride anions liberated as a consequence of these degradation reactions are commonly done, known as fluoride release rate, or FRR (also called fluoride emission rate, or FER). FRR has been proposed as an overall metric for quantifying membrane thinning, as the two have been reported to be directly correlated.277 Measuring FRRs is typically done by ion chromatography or ion-selective electrodes. In one example, Fouda-Onana et al.277 measured FRRs at the anode and cathode effluent water of a PEMWE cell operating at 60 °C and 80 °C. Substantially higher FRRs were observed at the higher temperature as well as in the cathode effluent water, which was attributed to crossover O2 reacting to form H2O2 in the presence of the platinum catalyst. Simpler ways to measure radical-induced degradation may exist, as Marocco et al.293 found a linear relationship between FRR and water conductivity by using a simple conductivity meter. This approach may be a way to monitor radical-induced degradation at scale, though it would require removing or quantifying other contributors to water conductivity.
Over time, radical-induced degradation could become significant enough to thin the membrane severely, exacerbating gas crossover and potentially causing electrical shorting. However, a wide range of outcomes are reported for the magnitude of radical-induced membrane degradation. For example, Grigoriev et al.213 reported that membrane thickness was reduced by 75% over 5500 hours. Another study294 loosely accredited the observed 35 μV/h degradation rate to ionomer degradation (attributed to increased HFR). These results contrast with other studies where membrane degradation is not observed or is minor.270,271 To reduce the possibility of contradictory conclusions, researchers must minimize the impact of degradation from all other cell components (e.g., the PTL or anode CL). It should also be noted that the degradation impact of different operation protocols (e.g., low current, high current, load cycling) is an area of active study and may contribute to discrepancies in rates of radical-induced degradation.
Mitigating radical-induced degradation in PEMFCs has been achieved through 1) fluorinating the end groups of ionomers (currently standard in PEMWE membranes such as N115) and 2) including radical scavengers (cerium/manganese-based) in the MEA. Although radical scavengers have been reported to have benefits in PEMWEs,295 they also have been attributed to catalyst poisoning and increased mass transport overpotentials.296 Recombination catalysts may limit chemical degradation by lowering crossover gas concentration at the CLs (reducing potential routes to H2O2 formation), but their use has been reported to increase FRR in one study.295 Either way, improving the fundamental understanding of chemical degradation and the trade-off of implementing various mitigation approaches will be necessary to ensure successful GW-scale deployment.
4.3.5. Hydrocarbons
Hydrocarbon-based membranes have long been sought as an alternative to PFSA membranes due to their potential for lower gas permeability, fluorine-free chemistry, and lower cost.297 Most hydrocarbon ionomers consist of a chain of aromatic units linked by various functional groups (Figure 10b). Although hydrocarbon membranes have promising attributes that can improve PEMWE performance, challenges in manufacturing and durability must be addressed to meet system targets. This section will outline the main obstacles for hydrocarbon membrane deployment and the strategies to overcome them.
4.3.5.1. Water Uptake
Hydrocarbon ionomers tend to possess lower proton conductivity than PFSA ionomers given the same water volume fraction.298,299 One reason for this property is a result of their conductive groups (sulfonates) being connected to a rigid aromatic backbone, which resists phase segregation into conductive percolating pathways. Decreased dielectric screening and a lower degree of dissociation of the sulfonate groups also limit proton conductivity. As a result, greater water uptake is needed to achieve comparable ionic conductivity to PFSA ionomers (e.g., a prominent hydrocarbon ionomer—sPPS—has a water volume fraction of 70%, while N115 has 40%300). However, this increased uptake makes them more prone to mechanical damage.
Several mechanical issues from high water uptake arise from the membrane’s reduced dimensional stability, which increases delamination and embeds stress on the membrane structure.301 Additionally, since there are spatial restrictions in the PEMWE cell that dictate the allowable extent of expansion, residual stress can build up, particularly along edges and under differential pressure (especially for thin membranes).302,303 Furthermore, higher water uptake can decrease mechanical toughness and reduce the gas permeation advantage of hydrocarbons, as the gas permeability of water is much higher than that of the unhydrated polymer.304 Lastly, mechanical degradation can feedback into chemical degradation through factors such as 1) increased ionomer surface area for reactions, 2) thermal concentration in deformed areas, and 3) exacerbation of radical generation through increased gas crossover and embedded stress.305−310
Fortunately, strategies to alleviate water uptake issues have been found. The first strategy is to utilize membrane chemistries that require less water uptake to achieve a sufficient level of conductivity. For example, block copolymer-based hydrocarbon ionomers can efficiently aggregate conductive sites to lower the required water uptake (at some sacrifice of permeability) while maintaining conductivity.263 Second, reinforcements (that are strong and acid-resistant) can be added to reduce swelling as well as improve mechanical durability. Analogous to what has been applied for PFSA membranes, porous PTFE-based reinforcements have enhanced dimensional stability—and thus mechanical durability—for hydrocarbon systems.311,312
4.3.5.2. Radical-Induced Degradation
Though hydrocarbon membranes possess lower gas permeability than their PFSA counterparts, the significantly higher level of chemical degradation—due to the rapid hydroxyl attack of hydrocarbons—may offset this benefit.300,304,313,314 While one can slow this degradation with radical scavengers,315 the attack is excessively fast to the extent that chemical degradation is challenging to prevent without excessively compromising ionic conductivity.316 Thus, to successfully benefit from the advantages of hydrocarbons, researchers must carefully weigh their disadvantages. Given that radical attack might be too rapid to be effectively prevented using scavengers, novel strategies to bolster chemical resilience should be explored, such as 1) performing polymer repair, 2) incorporating interfacial PFSA layers (e.g., in the membrane-CL interface), and 3) localizing radical scavenging at points of generation (i.e., catalyst sites).315
Overall, when pursuing efforts to mitigate outstanding challenges of hydrocarbon membranes, care should be taken to ensure that strategies are mutually compatible (i.e., not causing harm to other system components). Additionally, the mitigation methods employed must be durable over the lifetime of the PEMWE, which can be challenging to test.
4.3.5.3. Hydrocarbon Binders
Although binders pertain to the CL and not the membrane, they will be discussed here as this section covers hydrocarbon ionomers as a whole. As discussed previously, hydrocarbon ionomers may offer some technical upside in membranes, but there is not an obvious benefit for binders. Thus, the development path for hydrocarbon binders will likely require significant efforts to meet performance targets.
Hydrocarbon binders suffer from a multitude of issues, including 1) kinetic inhibition, 2) sluggish mass transport properties, 3) poor mechanical and chemical stability, and 4) CL manufacturing difficulties. For kinetic inhibition, while both PFSA and hydrocarbon ionomers contain sulfonate groups that can adsorb—and subsequently block—catalyst sites, this phenomenon has been shown to be more inhibiting for hydrocarbons.318 This difference is attributed to the greater presence of sulfonates (since hydrocarbon ionomers require more to achieve comparable PFSA conductivities)319 and to phenyl group adsorption on catalyst sites.314,320,321 Regarding mass transport, binders must rapidly facilitate gaseous transport, as lingering gases could inhibit the HER and OER.230,324 While the lower gas permeability of hydrocarbons benefits membranes, it is detrimental for binders and leads to increased gas transport (i.e., mass transport) resistances.325−327 Poor mechanical stability is tied to higher water uptake, which reduces dimensional stability and toughness, while poor chemical stability is tied to higher levels of radical-induced degradation.328 Furthermore, delamination of the CL is more commonly reported for hydrocarbon binders, causing increased contact resistance and decreased catalyst utilization.329,304,314,331 Lastly, CL manufacturing is also an issue; while PFSA binders readily form percolating networks, hydrocarbon binders have been linked to blocked pores332,333 and electronically isolated networks, leading to higher mass transport losses and lower catalyst utilization.333−336
Although many issues hinder hydrocarbon-based binders, many research levers exist to improve their efficacy: 1) polymer structure/property optimization, 2) solvent system optimization, 3) interfacial engineering, and 4) alternative designs. Researchers can consider how structural properties—such as pore structure, thickness, and tortuosity—can be tuned to facilitate mass transport. Chemical properties, such as conductivity and water uptake, can also be adjusted to enable greater mechanical strength. Furthermore, varying structural motifs (e.g., phenyl groups, ketones) can lead to less catalyst poisoning, reducing kinetic overpotentials. Optimizing solvent system parameters (e.g., solvent type, solid ratio, I/C ratio) to ensure high dispersity is critical to fabricating a well-connected CL microstructure. Tuning the molecular weight of the binder could also help, as this property has been linked to aggregate formation and connectedness.337 Penultimately, interfacial engineering (e.g., between CL-PTL, CL-membrane, binder-catalyst, etc.) can be promising in combatting delamination and increasing interfacial contact.314,315,338 Lastly, alternative designs can be utilized, such as the ionomer-free PTE proposed by Lee et al.,224 or simply using PFSA binders with hydrocarbon membranes.315
4.4. Porous Transport Layer
The porous transport layer (PTL) is responsible for 1) facilitating water and oxygen gas transport, 2) providing electronic conductivity between the CL and BPP, 3) removing heat from the CL, and 4) mechanically supporting the membrane during differential pressure operation. For visualization, we encourage the reader to refer to Figure 1 and Figure 8. PTLs significantly impact voltage efficiency since electronic and water/oxygen transport through the PTL influences ohmic and mass transport overpotentials, respectively. Additionally, the CL-PTL interface has been found to influence catalyst utilization and, thus, kinetic overpotentials.339,340 All these factors underline the criticality of the PTL for PEMWE performance. One note is that PTLs primarily facilitate through-plane (i.e., perpendicular to the membrane) transport, as opposed to BPPs, where in-plane transport (i.e., parallel to the membrane) dominates. Based on this terminology, a distinction between a standalone PTL and an integrated PTL+BPP design (typically used to reduce part count) can be drawn, as only the area where bulk through-plane transport occurs is considered the PTL for integrated designs.
Regarding functionality, PTLs are often compared to carbon GDLs in PEMFCs. However, the oxidizing conditions (i.e., >1.23 V) of the PEMWE anode do not allow carbon to be used due to it undergoing corrosion at potentials greater than 0.2 V.8 State-of-the-art PTLs are made of titanium due to its stability under such conditions. Still, challenges of surface passivation (via oxidation) persist, which results in decreased electronic conductivity. The porous property of PTLs is due to the titanium being produced as felts, meshes, foams, or sintered powders.342 More recently, the addition of a microporous layer (MPL)—a more porous and less tortuous layer at the surface of the PTL—is being developed to improve CL-PTL contact, which can enable lower catalyst loadings and thinner membranes. Although several PTL types have been studied, the final choice for stack integration will not only depend on performance but also on cost and scalability.
4.4.1. Cost
PTLs contribute ∼20% of the stack cost, or $47/kW, when considered in a 1 MW system (Figure 7). However, through economies of scale at 1 GW/yr deployment, that cost can be essentially halved to ∼$25/kW.149 Another significant cost lever is mitigating PGM usage for coatings. For passivation protection, PTLs are currently coated with platinum and iridium, which significantly adds to material costs. Given the limited understanding of degradation mechanisms, coatings are currently overengineered to ensure durability.162,134 Considering even a modest platinum coating of 0.1 mg·cm–2, the material alone can exceed $1.5/kW (assuming Pt cost is $50/g).
Aside from initial material costs, there are significant expenses for managing and refining materials. Each instance of material handling can incur a substantial cost, which can be particularly daunting given the ambitious U.S. DOE target of $2/kg H2 by 2026. Fortunately, cheaper alternative base materials and non-PGM coatings have shown promise. For example, Stiber et al.346 demonstrated minimal degradation over 1000 hours using a stainless steel PTL with a non-PGM coating (Nb/Ti).
4.4.2. Development
The various stages of PTL development are shown in Figure 12. Step one involves structure development. PTLs can be created through 1) thermal sintering, selective laser sintering, or electron beam melting of titanium powders, 2) heat treatment-induced diffusion bonding of titanium fibers, 3) weaving or expanding titanium meshes, and 4) tape casting or vacuum plasma spraying titanium particles.347−349 The most common method is powder or fiber sintering. Morphological properties—such as porosity, particle size, and thickness—are controlled by tuning process parameters (e.g., laser power, rastering rate, temperature) and starting material properties (e.g., particle size). Lastly, morphology can be quantified using techniques such as X-ray tomography,350 mercury intrusion porosimetry,351 or optical profilometry.225 The influence of structure on performance is discussed in the next section.
Figure 12.
PTL development stages. PTL structure (1) adapted from ref (352). PTL structures (2) and (3) adapted from ref (353). Copyright 2023 American Chemical Society. PTL coating figure adapted from ref (194). Copyright 2021 The Authors under Creative Commons Attribution 4.0 License (http://creativecommons.org/licenses/by/4.0/). SEM micrograph and uncoated vs. coated PTL durability figure adapted from ref (355). Copyright 2021 The Authors under Creative Commons Attribution 4.0 License (http://creativecommons.org/licenses/by/4.0/). Interface characterization figure adapted with permission from ref (356). Copyright 2020 Elsevier B.V. Techno-economic data adapted from ref (149). Copyright 2019 National Energy Renewable Laboratory (NREL).
Step two is the development of PTL surface coatings for corrosion resistance. State-of-the-art materials for coatings include precious metals such as platinum, gold, and iridium. Coatings will be discussed extensively in Section 4.4.7. Afterward, characterization is done in Step three to benchmark activity and durability. The authors recommend examining how PTL-related properties (e.g., porosity, tortuosity, thickness, CL-PTL interfacial contact, membrane delamination into the PTL, etc.) affect performance during this step.
Transitioning from lab-scale to industrial-scale, step four is manufacturing optimization for large-scale deployment. Although impressive morphological control can be achieved in lab scales, scaling up manufacturing (e.g., deploying roll-to-roll methods or creating batches >1000 cm2) can present quality control difficulties. Two methods are usually employed for large-scale manufacturing: 1) sintering—which involves combining, compacting, and sintering titanium powder, binders, and lubricants together, and 2) tape casting—which entails casting a titanium slurry into a thin layer, followed by drying and sintering. Tape casting provides precise control of sheet thickness and surface quality.348 For effective manufacturing, in-line quality control systems are necessary to guarantee morphology specifications and remove defective parts. Specifically, surface quality, presence of impurities, undesired edge warps or burrs, and inhomogeneous morphology need to be inspected. Failing to address these manufacturing-level defects can result in stack-level failures that are much more expensive to address. Creating quality compliance standards and methods to identify defects are necessary research areas.
Lastly, step five is techno-economic evaluation. To maximize PTL market readiness, costs and manufacturing lead times should be minimized. Significant cost reductions can come from using non-titanium base materials and reducing PGM usage for coatings. However, even if such improvements do not come to fruition, cost reductions can be achieved with higher production rates.149 As mentioned previously (Figure 7), costs can be essentially halved from $47/kW to ∼$25/kW when going from MW to GW scales.
4.4.3. Structure-Performance Relationships
Several studies have evaluated various PTL structures/types and their effect on PEMWE performance. Apart from sintered powder and titanium fiber PTLs, researchers have studied meshes,357 expanded meshes,358 foams,359 as well as multilayered combinations of these.360 Each PTL type can result in different interfacial contact behaviors with the CL, depending on the form factor of the surface. For example, the interface formed via sintered powder PTLs differs from that formed via sintered fiber PTLs, resulting in different performances even if their bulk properties (e.g., porosity and mean pore size) may be the same. In a comprehensive review, Yuan et al.342 analyzed the impact of PTL morphology on cell voltage and current densities (using sintered titanium powder PTLs). The results reveal a scattered relationship between mean pore diameter and voltage (Figure 13a). This scatter could be attributed to variations in test parameters among the different studies (e.g., temperature, pressure, and membrane thickness); nonetheless, a weak logarithmic correlation was observed, indicating that smaller pore sizes may decrease cell voltage. When examining porosity vs. cell voltage (Figure 13b), higher porosity was loosely correlated with decreased voltage, but only at the lower current densities of 0.2 A·cm-2 and 1 A·cm–2. At 2 A·cm–2, no correlation was clear.
Figure 13.
PTL structure–performance relationships. Mean pore diameter (a) and porosity (b) vs. cell voltage at 0.2, 1, and 2 A·cm–2 (for single-layer sintered titanium PTLs). Adapted with permission from ref (342). Copyright 2022 Royal Society of Chemistry.
4.4.4. Catalyst layer-PTL Interface
The catalyst layer-PTL (CL-PTL) interface is vital for PEMWE performance, especially under low loadings (as discussed in Section 4.1.1). The interface can be analyzed by calculating the interfacial contact resistance (ICR), which is influenced by contact pressure and deformation between the CL and PTL. For example, Yuan et al.342 calculated ICR as a function of contact pressure and density of interfacial contact points. To directly estimate electrochemical performance, one can measure the triple phase contact area (TPCA), which quantifies the area common to the catalyst, ionomer, and PTL. Higher TPCAs result in higher catalyst utilization and lower kinetic overpotentials. Kulkarni et al.339 took this concept further and calculated ECSA with TPCA values obtained through X-ray computed tomography (CT). Using a fiber PTL and low iridium loadings (0.05–0.1 mg·cm–2), Peng et al.177 observed that very low TPCAs resulted in limited electronic conductivity while very high TPCAs limited water accessibility to the CL (due to the catalyst particles being buried under the PTL fibers). Hence, for fiber PTLs with low iridium loadings, the lowest kinetic overpotential was observed at intermediate TPCAs between 29.4–35.4%, corresponding to a PTL porosity between 60–62%. Higher catalyst utilization was also shown to reduce mass transport overpotentials, as higher utilization provides well-connected pathways between the CL and PTL for oxygen transport. Work by Schuler et al.178 emphasizes this point by showing that mass transport limitations were more related to catalyst utilization than bulk mass transport.
Many modeling techniques have aimed to optimize the CL-PTL interface, given its importance in overall PEMWE performance. The types of models used include one-phase flow, two-phase flow, image-based, and stochastic. A single-phase (water) 1D model was developed by Ma et al.362 to simulate the effects of PTL pore size (at the interface) on catalyst utilization. A single-phase model sufficed since they focused on kinetically dominated regions, where two-phase flow effects can be assumed negligible. They found that smaller PTL pores at the interface and better in-plane electronic conductivity in the CL improve catalyst utilization. A two-phase 3D model developed by Weber et al.363 investigated membrane hydration and catalyst utilization underneath PTL land and pores. The model showed 1) low catalyst utilization underneath PTL pores due to poor in-plane conductivity and 2) local dry-out of the membrane under PTL land with increased current density (Figure 14). Sepe et al.364 recently developed an image-based multiscale modeling method that uses X-ray CT images to resolve the PTL microstructure for use in two-phase flow simulations. Using these simulations, the model generates macroscale parameters—such as relative permeability and capillary pressure-saturation curves—to predict PEMWE performance. They found that the PTL with small pore sizes, a narrow pore size distribution, and the highest area of water-oxygen contact performed the best. They explained that smaller pores require less pressure for oxygen to enter, leading to lower mass transport losses. Lastly, Lee et al.379 used a stochastic pore network model to optimize reactant transport and interfacial contact. By tuning porosity and particle size, their results showed an optimized PTL with a porosity of 26.5% and a powder diameter of 25 mm under “normal” operation (exact operating conditions were not specified). Overall, much insight can be gained from the numerous CL-PTL interface models in the literature. However, future models need to include catalyst loading effects, as CL-PTL interfacial contact can suffer dramatically at low loadings.
Figure 14.
Contour plot showing membrane hydration underneath a single circular pore at two current densities. The streamlines represent contributions of water flux from electro-osmotic drag (blue) and diffusion (red). “cCL” denotes cathode catalyst layer and “aCL” denotes anode catalyst layer. Adapted from ref (363). Copyright 2023 American Chemical Society.
Significant CL and membrane delamination can occur at the CL-PTL interface, resulting in electronically isolated catalyst islands that may not contribute to the OER (as discussed in Section 4.1.1).154 This effect is magnified under low loadings where fewer catalytic sites are available.178,180,367 Schuler et al.367 examined CL deformation after cell operation and observed microcracks caused by stress imposed by the PTL (Figure 15a). The cracks formed below the fibers (highlighted in green) do not impede electronic conductivity since no PTL void space is present. However, the cracks formed in the PTL void space (highlighted in red and yellow) do interfere with in-plane electronic conductivity, resulting in higher resistances. Furthermore, with differential pressure operation, CL/membrane creep into PTL surface pores can become severe and propagate existing cracks in the CL. Over thousands of hours, creep can result in pinhole formation, especially when thin membranes are paired with PTLs with highly porous surfaces. A recent study by Ferner et al.369 employed nano X-ray CT and pFIB-SEM to investigate how CL structure changes over time. The study observed that 1) CL thickness decreased (Figure 15b), and 2) CL regions compressed by PTL fibers (i.e., areas under and directly between PTL fibers) exhibited significantly different porosity and pore sizes compared to CL regions in the PTL pores (Figure 15c). The compressed areas had a 20% decrease in porosity (∼41→51%) and a 50% decrease in maximum pore size (∼600→300 nm).
Figure 15.
Membrane and catalyst layer deformation due to PTL compression. (a) Top: post-operational SEM images of the anode catalyst layer (CL) surface. Bottom: schematic of anode CL deformation. Compression fractures (yellow), tension-induced microcracks (red), and microcracks under PTL fibers (green) are shown. Cracks formed under PTL fibers do not impede electronic conductivity since no PTL void space is present. Adapted from ref (367). Copyright 2019 The Authors under Creative Commons Attribution Non-Commercial No Derivatives 4.0 License (http://creativecommons.org/licenses/by-nc-nd/4.0/). (b) 3D visualizations and 2D through-plane cross sections showing thickness distributions for a (i) pristine spray-coated CL, (ii) pristine blade-coated CL, and (iii) post-operational blade-coated CL. Images obtained using X-ray nanotomography. (c) CL porosities (i) and pore size distributions (ii) in a pristine PTL, in PTL pores, and under PTL fibers. Adapted from ref (369). Copyright 2024 The Authors under Creative Commons Attribution 4.0 License (http://creativecommons.org/licenses/by/4.0/).
Optimizing CL-PTL interfacial properties—perhaps even more so than bulk PTL properties—will be essential for reaching high-performing low-iridium loading PEMWEs. Lopata et al.340 revealed that interfacial properties, including pore diameter and titanium grain sizes, substantially impact catalyst utilization at low loadings and confirmed that interfacial pore properties were more influential than bulk pore properties. Novel methods can be explored to improve interfacial properties of the PTL, such as laser ablation, pore patterning, and laser-induced structuring.225,371,372
4.4.5. Mass Transport
Establishing efficient water transport and oxygen removal is important for high performance. Ambiguities have arisen in the definition of “mass transport losses,” with the term often used to broadly encompass residual losses not associated with kinetic or ohmic overpotentials. However, we will exclusively use the term to refer to losses associated with water and gas transport. Efforts to characterize mass transport in the PTL include operando X-ray imaging,371,373 neutron imaging,375,376 optical imaging,377 and numerical modeling,378−380 all of which have provided invaluable insights on maximizing performance.180,346,381
The formation of oxygen bubbles can critically impede CL function and has been associated with mass transport losses.375,383 Such losses are more significant under low loadings and high current densities,175,177,225 where the increased amount of evolved oxygen gas could mask the already limited number of reaction sites. In their modeling study, Moore et al.383 found that mass transport losses can be caused by discrete transient events of catalyst site blockage by oxygen bubbles, even though gas saturation does not significantly affect liquid saturation across the CL. Bubble formation comprises three stages: nucleation on the CL surface, growth to a critical radius, and detachment. Lee et al.375 identified a “critical current density,” where a sudden increase in gas saturation—and subsequently mass transport overpotential—occurs. They were able to increase the CCD by increasing the water flow rate, suggesting that there is a minimum flow needed for efficient oxygen bubble removal, as seen in Figure 16.375 Regarding heterogeneity, bubble accumulation can lead to current density and temperature maldistributions. Fortunately, optimizing the gas transport properties of the PTL can mitigate the aforementioned detrimental effects.
Figure 16.

Neutron imaging of oxygen content in PTLs at different flow rates and current densities. A general schematic of the imaged region is shown at the top. Three oxygen profiles under various flow rates are shown in (a–c). The bottom of each image represents the CL-PTL interface, while the top represents the PTL-BPP interface. Adapted with permission from ref (375). Copyright 2020 The Authors under Creative Commons BY-NC-ND 4.0.
PTL gas transport can be enhanced by tuning wettability or optimizing PTL porosity and tortuosity.177 Increased wettability has been shown to promote oxygen removal. Zhao et al.386 treated a PTL to increase its hydrophilicity and found increased activity compared to a control PTL. Furthermore, lower gas saturation was found in the treated PTL (through neutron imaging). Developing PTLs with higher porosity and lower tortuosity has shown reduced mass transport losses.177 However, the balance of mass transport and interfacial contact needs to be carefully tuned, as studies have shown an inverse relation between the two (at loadings <0.1 mgIr·cm–2).177 Aside from developing new PTLs, modifying existing PTLs is another approach for enhancing gas transport. Lee et al.371 demonstrated that creating perforations promotes faster gas removal and water intake. While having perforations present all the way through the PTL may negatively impact interfacial contact, Lee et al.225 showed that perforations that do not traverse all the way through can also improve mass transport without sacrificing interfacial contact. Efforts to reduce mass transport losses without compromising interfacial contact are required to achieve performance targets, and the authors foreshadow that MPLs may be a solution.
4.4.6. Microporous Layer
To improve CL-PTL interfacial contact, using a microporous layer (MPL)—a layer with smaller pore sizes than the bulk PTL—is proposed. Improving interfacial contact can lead to decreased mass transport and ohmic losses as well as increased catalyst utilization.
Numerous studies have examined the impact of MPLs on mass transport and ohmic losses. Using X-ray CT, Kulkarni et al.353 demonstrated that a thin (∼20 μm) MPL on a PTL allowed for 20% increased interfacial contact compared to a baseline PTL, improving mass transport properties. During a 1000 hour stability test where the current was held at 1.8 A·cm–2, this MPL showed a >100 mV performance improvement and a lower degradation rate compared to the baseline PTL (at both catalyst loadings of ∼0.1 mgIr·cm–2 and ∼2 mgIr·cm–2). In a pioneering attempt to develop MPLs, Lettenmeier et al.389 vacuum plasma sprayed fine titanium powders (grain size <45 μm) on sintered titanium powders. The resulting structure showed a clear bilayer, with the MPL and bulk PTL possessing pore sizes of 1.3 mm and 17 mm, respectively. The MPL resulted in marked ohmic improvement compared to the non-MPL, with a staggering HFR reduction of 20 mΩ·cm2. Following that, Kang et al.390 developed two MPL types, a microporous MPL using ∼5 μm particles and a nanoporous MPL using 30–50 nm particles. Interestingly, they found that the microporous MPL outperformed the nanoporous MPL (20 mV reduction at 2.0 A·cm–2) due to increased pore access for oxygen and water.
The role of MPLs for improved catalyst utilization has also been investigated. As stated in Section 4.1.2, conductive catalyst supports are currently lacking; thus, providing in-plane electronic conductivity between catalyst particles—and hence high catalyst utilization—at low loadings will likely depend on the PTL surface. MPLs will likely be critical at low loadings, where poor in-plane electronic conductivity could result in fatal losses in catalyst utilization. Schuler et al.180 constructed PTLs with MPLs of various pore sizes and studied their effect on catalyst utilization, albeit at higher loadings (2 mg·cm–2). The PTL structures are displayed in Figure 17a and polarization curves are displayed in Figure 17b. The bulk PTL had a mean pore diameter of 27 mm (the single layer “SL” sample has no MPL), and MPL 1, 2, and 3 had mean pore diameters of 6, 11, and 13 mm, respectively. Overall, catalyst utilization for the MPL samples increased by a factor of 2.2–2.8 compared to the SL sample, leading to ∼60–100 mV reductions in overpotentials at 2 A·cm–2. These voltage improvements were attributed to kinetic and mass transport improvements.
Figure 17.
Effect of different microporous layer (MPL) structures on performance. (a) The left figure portrays a generic MPL-containing PTL structure, while the right figures portray the MPL and single-layer “SL” (which has no MPL) structures. MPL 1, MPL 2, and MPL 3 differ in pore size and porosity. (b) Polarization curves for SL, MPL 1, MPL 2, and MPL 3; obtained using commercial Greenerity MEAs (Nafion N115 membrane) at 50 °C and ambient pressure. Adapted with permission from ref (180). Copyright 2019 WILEY-VCH Verlag GmbH & Co. KGaA, Weinheim.
4.4.7. Coatings
Coatings can help prevent surface oxidation and maintain CL-PTL conductivity. As such, coated PTLs have been shown to have increased performance and lower degradation rates than uncoated PTLs.8,161 Platinum is the most widely used coating material in commercial and academic research. Bernt et al.194 examined the impact of PTL coatings on cell performance and found that platinum coatings provide the necessary in-plane conductivity that low-loading CLs severely lack. MPL usage at low loadings (∼0.27 mgIr·cm–2) resulted in HFR reductions of over 15 mΩ·cm2, resulting in a ∼50 mV improvement in cell voltage at 3 A·cm–2. Rakousky et al.394 conducted a steady-state durability test for over 1000 hours and found that a platinum-coated PTL had an 89% reduction in degradation rate (108 → 12 μV/h) when compared to an uncoated PTL.
Coating degradation—caused predominately by metal dissolution and delamination—is heavily influenced by the application technique. Two widely used methods are electroplating and sputtering. Though electroplating is faster and simpler, it has uniformity and adhesion issues. In contrast, sputtering provides superior quality and precision (for a desired thickness and material amount) but requires longer times and more costly equipment. As a result, coatings from sputtering exhibit prolonged durability even after prolonged usage. Regarding material selection, some studies suggest that iridium is a better coating than platinum because of improved stability and higher conductivity of its oxides.395,396 Moreover, since the iridium sits at the CL-PTL interface, it can offer OER assistance to the anode CL or even enable ionomer-free CLs. Thus, some argue that the benefits of iridium coatings outweigh the additional costs imparted to the stack. Alternative techniques for surface modification include using novel mixed metal oxide coatings397 and acid etching,398 both of which enhance corrosion resistance. Although mixed metal oxide coatings show promise, their long-term durability is yet to be shown. Acid etching results in titanium hydride subsurface layers on the PTL, which does not affect electronic conductivity, but enhances corrosion resistance by mitigating titanium oxide formation.399
4.5. Gas Diffusion Layer
The gas diffusion layer (GDL) is the cathode-side equivalent of a PTL and is responsible for thermal conduction, electronic conduction, and hydrogen removal. However, the cathode is a low-potential environment, and thus, corrosion is not a concern during operation. Due to similarities in property and function, PEMWE GDLs have generally been adopted from PEMFC GDLs with minimal modifications.400−403 Current industrial GDLs (such as those from AvCarb, Freudenberg, and Toray) are carbon-based and are usually made from felts, papers, or woven substrates. This combination of material composition and structure makes GDLs compressible, unlike PTLs. Thus far, few works exist that study the impact of the GDL on PEMWE performance, since unoptimized GDLs adopted from PEMFCs have proved more or less adequate. This ease of incorporation is due to low HER overpotentials (relative to OER) and high H2 gas diffusion rates (relative to O2 gas and water).
4.5.1. Compression
Since GDLs are compressible, they are responsible for stress absorption from anode-related stress (since the PTL is incompressible) and membrane swelling. Compared to PEMFCs, the membranes used in PEMWEs are thicker, resulting in greater swelling and inducing additional stress on the GDL. Aside from stress absorption, GDL compression can also help prevent water flooding and promote BPP-GDL and GDL-CL electronic contact. Since hydrogen diffusivity is high, reductions in porosity due to compression should not significantly impact H2 removal. However, GDLs can experience mechanical damage due to overcompression if the cell is not properly designed or gasketed.
On the other hand, GDL decompression can also be an issue, which can result if hydrogen at the cathode is being compressed. Such decompression can lead to increased contact resistances and, thus, greater ohmic overpotentials. Generally, the frame that hosts the anode and cathode components in PEMWEs is made to a specific thickness, but manufacturing complications sometimes prevent the components from taking up the desired thickness. To combat the possibility of decompression, a thick layer (up to several mm) of stiff carbon is added in the cell. For PEMFCs, optimal GDL compression sits at around 10–25%; this range provides mechanical stability and effective transport.403 However, optimal GDL compression for PEMWEs cannot be generalized as it will depend on the cell configuration (e.g., membrane thickness, flow field design, etc.).
4.5.2. Wettability
Since water diffuses through the membrane to the cathode via electro-osmotic drag (Figure 1), a diluted hydrogen and water mixture ends up in the cathode outlet stream. Thus, hydrophobic GDLs are desirable as they mitigate water transport from the membrane into the outlet stream, resulting in pure hydrogen (also called “dry hydrogen”). Hydrophobicity can be attained using a hydrophobic base material or by incorporating a hydrophobic MPL into the GDL. PTFE is currently used as a hydrophobic additive, but it is not electronically conductive and thus contributes to higher BPP-GDL interfacial contact resistances. Therefore, finding alternative materials to promote hydrophobicity could be a promising research area.
4.5.3. Outlook
Although research is still needed for GDL optimization, existing designs derived from PEMFCs will be sufficient for GW-scale deployment. However, one difference to consider is that PEMWE GDLs are usually created at high temperatures in vacuum furnaces to eliminate impurities, as PEMWEs are more sensitive to cation contamination than PEMFCs. This additional step can increase manufacturing costs. However, this step may not be necessary as its impact on long-term performance has not yet been studied. Lastly, it should be considered that although GDL corrosion is typically not a concern, PEMWE shutdown events can lead to rapid carbon corrosion due to the presence of reverse currents. Thus, care should be taken to ensure that PEMWE durability is not affected by excessive GDL corrosion.
4.6. Bipolar Plate
Bipolar plates (BPPs) are expensive due to material needs and the manufacturing process, contributing 15–50% of the total stack cost.150,405,406 BPPs are responsible for mass transport (H2O in, H2 and O2 out), electronic conduction, heat conduction, and mechanical support.150,407−45 Unlike PTLs, which are responsible for through-plane mass transport via diffusion, BPPs are responsible for in-plane mass transport via convection (through their flow fields). As shown in Figure 18a, they are called “bipolar” because one side is in contact with the anode, and the other side is in contact with the cathode (unless they are located at either end of the cell/stack).407 For BPPs to be effective, they must possess low contact resistance and efficiently transport water and gases. Furthermore, just like the PTL, BPPs need to be made of a corrosive-resistant material that can withstand the acidic and oxidizing conditions of the PEMWE anode.
Figure 18.

(a) General schematic of a two-cell PEMWE stack, with the placement of the three bipolar plates highlighted. In this setup, only the middle bipolar plate is in contact with both the anode and cathode. (b) Examples of bipolar plates made of (i) titanium, (ii) stainless steel, and (iii) stainless steel coated with a Au/Ti mix. Adapted with permission from ref (411). Copyright 2014 IOP Publishing.
The most common base materials for BPPs are titanium and certain stainless steels (SS; e.g., SS316 and SS403), as shown in Figure 18b (i) and (ii).150,407 Unlike for PEMFCs, graphite is only suitable for the cathode environment.45 With the use of titanium or SS, coatings are needed to maintain low interfacial contact resistance with adjacent components. For SS specifically, the coating would also need to provide corrosion protection. Precious metals such as platinum, gold, and silver are typical coating materials—as shown in Figure 18b (iii)—with platinum being the most common.405,407 To apply these coatings, electrical plating is conventionally used, but methods such as physical vapor deposition are in development.
Overall, the primary limiting factor for scale-up is cost. Developments for PEMWE BPPs can leverage knowledge acquired from PEMFCs, but material limitations provide challenges.405,407 Fortunately, manufacturing techniques and flow field designs from PEMFCs can be adapted with relative ease.
4.6.1. Flow Field
BPP flow field design influences heat conduction and mass transport in PEMWEs. Since excess water flows throughout the cell for heat removal, flow fields must equally distribute this water to avoid hotspot formation. Additionally, the pressure drop across flow fields should be minimized to reduce pumping costs.
Many methods can be employed to create a flow field, such as electroetching, stamping, electrical discharge machining, electrochemical machining, electroforming, and additive manufacturing.412 Three types of flow field structures exist: 1) Multilayered, where layers of a metal mesh or screen are stacked on a flat base material (Figure 19). Pores of adjacent layers are offset to construct a 3-D hollow structure for water and gas transport. Pore sizes and the number of layers are critical design parameters. 2) Electroetched, where serpentine flow field channels are etched on a thick metal plate. This method simplifies the BPP manufacturing process as only one component is needed, but the method suffers from high processing costs. 3) Stamped, where 3D flow structures are stamped onto a base. Stamping onto thin base materials (∼0.5 mm)—especially stainless steel—is common for PEMFC BPPs.412−415 This stamping strategy has been shown to enhance mass transport.416 Like the etched structure, assembly costs are reduced due to only needing one component. However, complications arise from difficulty controlling stress distortion. Improper stress control during stamping could result in uneven surfaces and, ultimately, complications in stack sealing (especially under high pressures).
Figure 19.

Example of a bipolar plate flow field design consisting of multilayered metal screens. 12A, 12B, 14A, and 14B are separate layers with different diamond patterns used to form an optimized structure for water and gas flow. Adapted from ref (417).
Flow field performance is a strong candidate to be improved through modeling. Distribution profiles of oxygen, pressure, temperature, current density, and fluid velocity (Figure 20) can be constructed for various flow field types.418−421 These simulations require Multiphysics models that couple heat, mass, and charge transfer effects. Furthermore, two-phase flow effects through other cell components (like the PTL) must be included for comprehensiveness. Olesen et al.422 modeled three circular interdigitated flow field variations. Reasonably, the regions with the highest temperature and oxygen content had the highest current densities. Interestingly, despite the similar overall performance, they found significant in-plane variation in temperature and current density between the three designs. Another study421 compared a novel interdigitated-jet hole flow field design with two common designs (standard interdigitated and single serpentine). They found that the novel design had more homogeneous water distribution and more effective gas removal, leading to more uniform current density and temperature profiles. Qing Wei et al.424 used a similar model to compare a novel mesh flow field with commonly used parallel flow fields. They found that the mesh structure enabled greater temperature and current density uniformity (Figure 21) as well as lower energy consumption.
Figure 20.
Examples of different flow field architectures and their resulting velocity profiles: (a) parallel flow field, (b) serpentine flow field, and (c) point flow field. Adapted with permission from ref (420). Copyright 2022 Elsevier Ltd.
Figure 21.
Performance comparison between a parallel channel flow field (Model A) and a novel mesh flow field (Model B). Contour plots showing (a) current density (A·cm–2) and (b) temperature (°C) distributions. Adapted with permission from ref (424). Copyright 2023 Hydrogen Energy Publications LLC.
4.6.2. Coatings
BPP coatings must be stable in the highly corrosive environment of a PEMWE anode: oxygen-saturated, potentials around 2 V, temperatures ≤80 °C, and pH∼0 (Figure 22).406,408,45 Furthermore, they must have low contact resistance, high through-plane electronic conductivity, good adherence to the BPP, and scalable methods of deposition.406,408 Titanium BPPs are usually coated with PGMs, as they meet the requirements above and can also prevent surface passivation.45 If SS is used as the base material, the coating must also prevent ion leaching, which could lead to increased coating costs.406,408 However, SS is cheaper than titanium, and thus coated SS BPPs could still be cheaper than coated titanium BPPs.150,406 The method used to apply the coating could also influence costs; common methods include plasma, powder, and electrochemical deposition.427
Figure 22.

A schematic of the conditions relevant for bipolar plate (BPP) coating design. Adapted with permission from ref (406). Copyright 2016 Elsevier B.V.
BPP designs with novel coatings have also been demonstrated. Using a SS base, Gago et al.406 developed a two-layer coating consisting of a 60 μm titanium layer and a ∼1 μm platinum layer. The titanium provided corrosion resistance, while the platinum prevented the titanium from passivating. Future work dedicated to decreasing the titanium layer thickness can reduce coating costs.406 A different study by Rojas et al.408 concluded that utilizing a SS BPP with a multilayer Ti/TiN coating can reduce manufacturing costs by 90% compared to a titanium BPP. However, further work must be completed to make this technique more scalable.
4.6.3. Hydrogen Embrittlement
Hydrogen absorption can occur on the cathode side of BPPs due to high hydrogen pressures and radical generation from the HER, weakening the mechanical integrity of the BPP and leading to a phenomenon known as “hydrogen embrittlement.”428 Titanium BPPs can suffer mechanical failure with hydrogen concentrations over 8,000 ppm,429 and it was reported that such plates could absorb over 1000 ppm in 500 hours of operation (meaning that stack failure could occur in just 4,000 hours).429 Even using platinum coatings, hydrogen embrittlement can still occur since hydrogen can absorb in the platinum and form Pt–H bonds.431
Two approaches to prevent hydrogen embrittlement are applying a gold coating or a pinhole-free carbon coating to prevent direct contact with hydrogen. Gold can help prevent hydrogen absorption, but due to hydrogen’s high diffusion coefficient, a thick coating (>200 nm) is required. Such high precious metal usage presents cost issues. Another approach is to have a pinhole-free carbon coating, which has been shown to reduce hydrogen absorption.429 However, challenges lie in costs and processing difficulties associated with pinhole-free manufacturing. Lastly, a more roundabout strategy would be to allow the titanium surface to form surface oxides—which would prevent hydrogen absorption—and then partially cover the surface with gold dots to enable adequate electronic conductivity (Figure 23).432 It was shown that surface coverage of less than 10% with gold dots would meet contact resistance requirements. Overall, hydrogen embrittlement is still a significant issue and will require developing effective coating materials and scalable coating methods.407
Figure 23.

SEM photo of a titanium bipolar plate covered with gold dots to improve interfacial electronic contact. The uncovered surface is composed of a thick titanium oxide layer to prevent hydrogen absorption.
4.6.4. Outlook
Current BPPs are made of titanium coated with platinum, contributing up to 50% of stack costs. For PEMWE scale-up, the costs of the base and coating materials must be reduced. For the base, stainless steel is an attractive option; however, a coating that is inexpensive and durable (toward corrosion and ion leaching) is required. For the coating material, platinum can still be used, but loadings—which currently sit at ∼1–5 mg·cm–2—must be reduced to decrease costs.434 Of course, platinum-free coatings are ideal for cost reduction, but further work into their effectiveness and scalability is required. Lastly, hydrogen embrittlement presents a major durability issue and needs to be addressed with novel coating approaches.
5. AST Proposals
Accelerated stress tests (ASTs) are durability testing protocols that expedite the degradation of components under industrially relevant conditions. These tests are needed to estimate system lifetimes without numerous years of testing. Furthermore, ASTs can help us understand degradation under different operating regimes, which may be essential for industrial electrolyzers. For example, although current PEMWEs operate at constant loads to minimize degradation, techno-economic analysis indicates that dynamic operation following cheap renewable electricity (i.e., “load following”) will be critical to producing low-cost hydrogen.162 While numerous papers have examined PEMWE durability,48,272,436,438 no standardized AST protocols exist. This section will propose recommendations for such protocols to initiate the proccess of AST standardization.
The U.S. DOE has published various standardized ASTs for PEMFCs, including widely used component-level tests, as well as rarely used MEA-level tests (for overall system lifetime predictions).440 Their “Research, Development, and Demonstration Plan”440 lists ASTs for catalysts, catalyst supports, MEA chemical stability, membrane mechanical stability, membrane chemical/mechanical stability, and drive-cycle durability. While the first five tests target specific components and have been widely used in the literature, the last AST (“drive cycle durability protocol”) targets overall system durability (under light-duty operating conditions) and has rarely been reported.267,441 Since lifetime predictions are highly dependent on the exact duty cycle used in any particular application, it is more common for overall system ASTs to be specially developed by original equipment manufacturers (OEMs).
Partnerships between OEMs and researchers can facilitate durability improvements. OEMs can provide researchers with end-of-life materials and data pointing to specific failure modes, so that efforts are not misappropriated to irrelevant degradation concerns. At the same time, researchers can use their resources to understand the fundamental issues governing degradation. Given the criticality of meeting lifetime targets, researchers must prioritize the expansion of testing capacities (both ex situ and operando) to probe durability topics and perform ASTs.
Although less standardized, PEMWE ASTs have been proposed for the anode, cathode, and overall system. The EU published a harmonized report on electrolyzer testing and found the “key stressors” for PEMWE durability to be temperature, pressure, water flow rate, and water quality.443 Using these four stressors, eight ASTs were developed for the anode and cathode. Two overall system ASTs were also proposed: a “reactive” test with 1 min step intervals and a “flexible” test with 15 min step intervals (each step was a current hold, ranging from 25–200% of nominal current density). Moreover, Aßmann et al.444 proposed overall system ASTs based on different operating modes: low load, high load, dynamic load, and startup/shutdown. While a handful of overall system ASTs have been proposed, component-specific tests are lacking. Here, we propose ASTs for each cell component, summarized in Table 3. The x/y notation (e.g., H2/air) signifies that x is in the anode and y is in the cathode.
Table 3. Proposed Component-Specific Accelerated Stress Tests (ASTs) for PEMWEs.
| component | proposed AST | specifier |
|---|---|---|
| Anode catalyst | 1.45–2.0 V cycling | Standard Operation |
| 0.5–2.0 V cycling | Start/Stop Operation | |
| Cathode catalyst | 0.5–2.0 V cycling | |
| Membrane | OCV in H2/air | Chemical Stability |
| 1–200 bar cycling in air/air | Mechanical Stability | |
| 1–200 bar cycling in H2/air | Overall Stability | |
| Porous transport layer | 2.0 V hold | |
| Gas diffusion layer | Air/H2 cathode cycling | |
| Bipolar plate | ex situ 2.0 V hold | ex situ |
| 90 °C operation | in situ |
Lastly, it should be noted that component-specific ASTs could produce undesired stress on other components, leading to seemingly contradictory results. For example, a study by Alia et al.137 found that dynamic loads cause more degradation than constant loads, while another study by Frensch et al.294 reported the opposite. However, performance losses were attributed to kinetic overpotentials in the first study and ohmic overpotentials in the second. Thus, care should be taken to meticulously probe the cause of electrochemical performance losses during ASTs (e.g., catalyst dissolution, membrane thinning, PTL/BPP passivation, etc.), regardless of which component is targeted.
5.1. Anode Catalyst Layer
PEMFC catalyst ASTs involve cycling between two potentials where platinum is in different oxidation states (metallic platinum and platinum oxide/hydroxide) and thus exhibits vastly different dissolution rates.445 This cycling results in catalyst agglomeration and loss of electrochemically active surface area.441 In addition to potential cycling, high temperature and relative humidity (RH) also accelerate degradation.446 Thus, the AST (for the cathode catalyst) is 0.60–0.95 V cycling (2.5 s holds) at 80 °C and 100% RH. Furthermore, the test is performed in an H2/N2 environment to prevent ionomer degradation.
PEMWE anode catalyst ASTs can be designed with a similar potential cycling strategy, as transitions to lower voltages and OCV conditions were shown to be highly degrading (Section 4.1.3). To assess durability representative of standard operation, 1.45–2.0 V cycling can be used; for durability representative of startup/shutdown operation, 0.5–2.0 V cycling can be used. For both tests, an elevated temperature of 80–90 °C can be used, and the potential hold time can be adjusted between 10–30 s. This time window allows for rapid cycling but also provides adequate time for iridium to undergo oxidation state changes. Electrochemical performance at kinetically dominated regions (i.e., at low current densities) can be used to track catalyst degradation.
5.2. Cathode Catalyst Layer
The durability of the cathode CL has drawn some attention regarding startup/shutdown operation. Grigoriev et al.237 reported significant platinum dissolution attributed to the 600+ shutdown events in their 4000 hour test. During shutdown, reverse currents can occur (i.e., the system works as a fuel cell) and trigger mechanisms of platinum dissolution until all electrolysis gases are exhausted (the authors suggest purging the anode and cathode gases as mitigation strategies).237 Voronova et al.448 also observed this degradation mechanism, as they found performance losses when cycling between 1.4–2.2 V, but not when cycling between 1.5–2.2 V.
Since shutdown conditions impart the greatest stress on the cathode catalyst, we propose the same test as the startup/shutdown AST for the anode catalyst: 0.5–2.0 V cycling. While OCV-load cycling has been seen in the literature for cathode degradation,234 we do not recommend incorporating OCV conditions in standardized protocols as reproducibility will likely be unsatisfactory. The nature of OCV conditions (i.e., how quickly the potential decays, what value the potential will decay to, etc.) will depend on the rate of hydrogen crossover, which can vary significantly with membrane thickness and chemistry.
5.3. Membrane
Membrane degradation has been identified as one of the main failure mechanisms for PEMWEs213,276,452 and was discussed extensively in Section 4.3.4. A summary of the two degradation modes—chemical and mechanical—will be presented here. Chemical degradation can lead to membrane thinning213 and occurs when radical species attack the PFSA ionomer (Figure 11). The rate of degradation can be quantified by measuring fluoride release rates (FRRs). A model by Chandesris et al.453 found that temperature accelerates FRRs and that higher rates are seen at the cathode. Moreover, current cycling was reported to cause increased FRRs compared to steady-state operation.294 Mechanical degradation as a failure mode has been demonstrated with thin N211 membranes (∼25 μm);455 membranes can experience mechanical stress through delamination or the formation of hotspots. It has been reported that thicker membranes penetrate 19–45 μm into the PTL, with factors such as membrane thickness and PTL porosity influencing the extent of penetration.178 Furthermore, flow field designs that lead to nonuniform H2O/O2 distributions across the cell can result in membrane hotspots that accelerate degradation.271
Three membrane ASTs for PEMFCs currently exist: OCV hold in H2/air (for chemical degradation), RH cycling (for mechanical degradation), and RH cycling in H2/air (for combined chemical/mechanical degradation).267,458 Since mechanisms of membrane degradation are similar between PEMFCs and PEMWEs, these ASTs can be adapted for PEMWEs. RH cycling can be replaced by pressure cycling, which is more relevant to electrolyzer operation. For chemical degradation, an OCV hold in H2/air at 90 °C and 30% RH can be performed. For mechanical degradation, pressure cycling between 1–200 bar (which covers relevant pressure ranges) in air/air at 90 °C can be done. For a combined chemical/mechanical test, the pressure cycling can be performed in H2/air. Lastly, a dual membrane and anode catalyst AST can be created by combining pressure cycling with the startup/shutdown anode catalyst AST: cycling between 1 bar/0.5 V and 200 bar/2.0 V. Catalyst degradation can be tracked via polarization curves, while membrane degradation can be tracked via HFR changes or hydrogen crossover rates.
5.4. Porous Transport Layer
As catalyst utilization/degradation heavily depends on the CL-PTL interface, developing durable PTLs will be critical. Surface passivation is a primary PTL degradation mechanism, leading to increased kinetic and ohmic overpotentials. Coatings can help mitigate passivation, but the coating itself is subject to degradation in the form of dissolution and delamination. Thus, since PTL durability is tied to surface passivation, a constant high voltage load of 2.0 V would be an appropriate AST. It should be noted that PTL degradation is intimately tied with catalyst degradation, so both should be evaluated in conjunction.
5.5. Gas Diffusion Layer
GDLs have been shown to corrode under the oxidizing conditions of PEMFC anodes,459,460 but their corrosion under the reducing conditions of PEMWE cathodes is typically not a concern. However, PEMWE shutdown events can lead to reverse currents and trigger carbon oxidation. Thus, if frequent shutdown events are implemented in an operating strategy, care should be taken to ensure that GDL corrosion does not significantly impact system durability. For an AST, since the GDL environment does not experience oxidizing conditions during regular operation, cathode cycling between oxidizing (air) and reducing (H2) environments could be used—as proposed by Perry et al.460
5.6. Bipolar Plates
Despite the BPP’s importance in durability and cost considerations, BPP ASTs have not been proposed for PEMFCs or PEMWEs. However, the U.S. DOE has published durability-related targets for PEMFC BPPs, including H2 permeation rates and corrosion resistance.440 To quantify corrosion resistance, ex situ tests are performed where corrosion currents are measured via chronoamperometry at relevant potentials in a simulated PEMFC environment—pH 3 with 0.1 ppm of fluoride anions (to represent membrane degradation products). It may seem logical to perform similar measurements for PEMWE BPPs, but currents are dominated by H2 and O2 evolution at relevant potentials (i.e., above 1.23 V or below 0 V). Nevertheless, an ex situ test can still be performed to examine ion leaching, H2 permeation, and contact resistance. The test can be performed at 90 °C, pH 3, 0.1 ppm of HF (for the fluoride anions), and +2.0 V (for anode conditions) or −0.2 V (for cathode conditions).
However, it should be stated that stack OEMs prefer to see in situ durability data for BPPs, which can be highly time-consuming to obtain. OEMs typically use their own protocols based on targeted operating conditions, but for a general in situ BPP AST, we propose an elevated operating temperature of 90 °C to accelerate corrosion and hydrogen embrittlement.
6. Industrial Perspectives
6.1. Nel Hydrogen
Nel Hydrogen is a global leader in deployed water electrolyzer systems, commercially selling liquid alkaline and PEM products worldwide. While anticipating the hydrogen economy to take shape, Nel has been fortunate to sell electrolyzers for industrial applications, such as generator turbines (cooling gas), weather balloons (filling), heat-treatment furnaces (atmosphere control), and other applications requiring a reducing environment. Along with a focus on continuous durability and electrical efficiency improvements, Nel has aimed to scale up devices to meet emerging industrial and energy storage markets for green hydrogen. As shown in Figure 24, significant opportunities exist for green hydrogen to decarbonize existing industrial processes.
Figure 24.

Overview of the current industrial hydrogen market and methods for hydrogen production.
Nel has supported the hydrogen economy by developing a broad portfolio of systems, spanning kWs to hundreds of MWs. The scale-up of equipment and devices not only enables market penetration into areas requiring tons of hydrogen generation per day, but also serves to reduce CapEx. Such CapEx reductions are critical to meet green hydrogen cost targets—such as $1/kg by 2031 (U.S. DOE)—and compete with hydrogen produced through SMR. Figure 25a depicts the two main pathways for cost reduction: 1) technological development, which includes factors such as lowering catalyst loadings and using thinner membranes, and 2) scale-up for large-scale production. Technological development offers significant opportunities for cost reductions, but economic returns gradually flatten as advancements are implemented. Fortunately, scale-up can provide further cost reductions, approximated by the rule of “six-tenths” (Figure 25b). According to this rule, for a given cost of an electrolyzer system (CA), if manufacturing capacities increase by a factor of X, the final cost (CB) decreases by a factor of X0.6.
Figure 25.
Graphical portrayals of cost reduction concepts. (a) Cost reductions through technological development and scale-up. (b) Rule of six-tenths as applied to electrolyzer systems. CA is the given cost of an electrolyzer system, X is the factor by which manufacturing capacities increase, and CB is the final cost. (c) Cost reductions via volume discounts and automation.
To enable scale-up, Nel has continuously worked to increase stack size in active area and cell count. Such increases have not always been easy due to limitations in the existing supply chain. The available form factor of existing components has often been a constraint dictating how large PEMWE systems can go, with stack configurations frequently forced back into the design space. However, with the scale-up of green hydrogen, this limitation is beginning to diminish. Thus, suppliers have recognized this time as an opportunity to expand their businesses and are open to developing their own manufacturing methods to address larger scales. This increase in supplier engagement has additional benefits related to cost: 1) the formation of supply chain agreements, which contribute to large orders and volume discounts, and 2) direct engagement in the design phase from suppliers, which leads to more conscious stack design tailored for automation. These concepts are illustrated in Figure 25c, with the blue plot showing cost reductions via supply chain agreements and the black plot showing cost reductions via automation, which includes the most rudimentary steps (such as gasket cutting) all the way to stack assembly.
As renewable electricity costs continue to decline, the acceptance of PEMWE systems is becoming more widespread and will continue to build momentum. The challenge is for us to utilize technological advancements, increase production scales, obtain supplier engagement, and implement high-volume manufacturing processes to position electrolysis as a cost-effective solution to help global decarbonization.
6.2. Undisclosed Company
Understanding the broader context of a hydrogen economy is essential when approaching PEMWE development. This includes aspects such as large-scale hydrogen production, storage, and distribution. A comprehensive pioneering initiative should involve green hydrogen production in an interconnected hydrogen-fueled ecosystem; a model of this concept is illustrated in Figure 26. In such a system, green hydrogen generated by PEMWEs is distributed across a connected infrastructure to power buildings, fuel both light- and heavy-duty fuel cell vehicles, and decarbonize industrial plants. Currently, since there is no significant market for green hydrogen, the demonstration and deployment of PEMWEs in an ecosystem would help build supply and demand. These demonstrations—such as the one in Fukushima462—can provide valuable information for understanding the technical feasibility and economic viability of green hydrogen. Additionally, such a demonstration serves as an invaluable testbed for assessing performance limitations and degradation over time, providing critical real-world data to refine PEMWE technology.
Figure 26.
Schematic of a green hydrogen ecosystem. Green hydrogen production, storage, transportation, and end use depicted.
The primary challenge for green hydrogen is reducing production costs.463,464 In addition to achieving economies of scale, there are three primary pathways to reduce costs: cheap electricity coupling (i.e., load following), material innovation, and PEMFC synergy. First, electricity prices are the single largest driver for overall production costs. Therefore, it is imperative to couple PEMWEs with low-cost electricity from renewable energy sources like wind and solar. Thus, dynamic operation of PEMWE systems needs to be optimized for minimal performance degradation.
Second, material innovation plays a pivotal role in cost reduction. The reliance on iridium, one of Earth’s rarest elements, presents a significant challenge. Developing catalyst materials with increased activity and stability is essential to meet efficiency, lifetime, and catalyst loading targets. Current commercial PEMWEs use a loading of ∼3 mgIr·cm–2; reducing this to 0.1 mgIr·cm–2 or less is critical to make large-scale deployment economically feasible.465 Furthermore, manufacturing MEAs with such low loadings presents significant challenges with existing coating methods, such as doctor blade coating or slot die coating. Thus, innovations in catalyst design and large-scale catalyst layer fabrication techniques are imperative.
Third, synergy with already established PEMFC technologies could also reduce costs. Many components in PEMWEs—including the cathode catalyst, membrane, and BPP—are common with those used in PEMFCs. A strategic synergy between these two technologies can accelerate the initial development phase and capitalize on economies of scale, leading to significant reductions in investment costs for PEMWEs. Moreover, the shared components can enable greater cost efficiencies—particularly in mass production—due to common supply chains and manufacturing processes.466
With combined efforts in material innovation, cost reduction, and real-world demonstrations, GW-scale PEMWE deployment can be achieved. Ultimately, demonstrating the technical feasibility and economic viability of a green hydrogen ecosystem is critical for PEMWE manufacturers to establish sustainable businesses.
6.3. Plug Power
PEMWE devices are rapidly moving from niche applications to projects greater than 100 MW. The United States has pledged $9.5 billion to hydrogen production hubs and electrolyzer research, while Europe is looking to add 40 GW of green hydrogen by 2030. This scale-up brings with it several challenges. First, the supply chain is not currently set up for these developments, and rapid production scaling could put pressure on precious PGM catalyst materials. The maturity of regulations, site permitting, and codes vary wildly by location, leading to difficulty in design standardization for global deployment. An influx of interest and money has led to thousands of new entrants, few with the experience and history necessary for large-scale projects. Lastly, with all this considered, safety must be at the forefront of system deployments.
Scaling up PEMWE systems requires a consistent supply of critical components, such as catalysts, membrane materials, and PTLs. Limited production capacities of these components can lead to bottlenecks, delays, and increased costs. Additionally, the demand for rare catalyst materials, especially iridium, can result in supply chain vulnerabilities. Fortunately, multiple studies have shown that iridium usage is low-risk, and PEMWEs can reach the terawatt level with decreased loadings, increased current densities, and iridium recycling.467,468 Another concern is the PFSA materials necessary for the membrane, binders, and gasketing. Bans on such materials are under consideration in both the European Union and the United States. Though there is active research in non-PFSA materials, nothing to date has shown adequate durability under realistic conditions (>50,000 hours at >60 °C).
Large-scale PEMWE projects must adhere to various codes and standards to ensure operational reliability and safety. These codes cover equipment design, installation, operation, maintenance, and emergency response. Such regulations are most mature in Europe, where stacks usually need to be ATEX certified (Atmosphère Explosible; “Explosive Atmospheres”; ensures safe use in explosive environments) and must obtain a CE mark (conformité européenne; “European Conformity”; affirms conformity with health, safety, and environmental standards). The interior of a stack is generally, and rightfully, considered an explosive environment, requiring ATEX certification. Afterward, to obtain a CE mark, the stack must meet the “Pressure Equipment Directive,” demonstrating that it can withstand a multiple of the maximum allowed working pressure. This process requires additional design, testing, and manufacturing certifications from notified bodies. In the U.S., it is generally left to local regulatory bodies who often rely on ASME (American Society of Mechanical Engineers) standards. Predictably, this flexibility leads to wildly varying permitting needs and timeframes. Only recently was a unified path being created for an electrolyzer certification scheme—called “U stamp”—for stack quality and engineering requirements, developed through an ASME case code.
Scaling up PEMWE systems involves compliance with local, regional, and national regulations. Obtaining hydrogen production, storage, and transportation permits can be complex and time-consuming. A good starting point for understanding the hundreds of codes and requirements from the stack to the system level is reviewing the guidelines for the United Kingdom and the U.S. state of California.469,470 Zoning restrictions, environmental impact assessments, and public safety must be considered. Collaborative efforts between industry stakeholders and regulatory bodies are necessary to streamline permitting procedures and ensure efficient project execution. Commonality is critical to bringing hydrogen generation to multiple locations, as regulatory uncertainty can defeat promising projects before they begin. R&D is also vital for scale-up: innovations in catalyst loading reduction, non-PFSA ionomers, energy efficiency, system design, safety measures, and supply chain optimization can collectively alleviate the difficulties associated with large-scale implementation. Public-private partnerships, academic collaborations, and government support are actively being pursued in these areas, with targets established for cost and performance to bridge efforts together.242
As the scale of PEMWE systems increases, so do safety concerns. Hydrogen, though a clean fuel, is highly flammable and poses explosion risks. Inadequate handling and storage of hydrogen can result in catastrophic accidents. Proper personnel training, stringent safety protocols, leak detection systems, and robust ventilation infrastructure are imperative, especially in large-scale installations. Although codes and standards exist for stacks and systems, they are often overlooked due to their immaturity or inconsistency between locations. Safe stack operation requires constant monitoring of voltage, water flow, temperature, pressure, and—most importantly—hydrogen content (on the anode side). However, even with constant system monitoring, stack designers must plan for worst-case scenarios. As an example, Plug Power tests all system components for catastrophic failure; Figure 27 shows the time-evolved progression of one of these tests, where a 1 MW stack and its anode outlet are subjected to worse-case H2/O2 stoichiometries that could result during a complete failure (i.e., membrane rupture). The H2/O2 gas mixture is then detonated, and the system is observed to ensure that physical explosion risks are contained and that the stack maintains its physical integrity. To avoid premature ignition, one must remove the catalysts in the stack before testing. Similar tests are done on the H2O/O2 separator, which is generally the system component with the most significant potential for explosive damage.
Figure 27.

Testing of stack detonation under worst-case H2/O2 stoichiometric conditions. Test ensures that the stack contains the explosion and that no shrapnel is generated upon failure.
Scaling up PEMWEs holds the key to unlocking hydrogen’s potential as a clean energy carrier. However, challenges related to supply chain management, safety considerations, permitting procedures, and adherence to codes and standards must be effectively addressed. Collaboration among stakeholders, regulatory bodies, researchers, and industrial companies is essential to overcome these challenges and pave the way for a sustainable and efficient GW-scale PEMWE industry.
7. Outlook
To reach net zero emissions, PEMWE deployment must scale up tremendously from 0.3 GW to 220 GW by 2030. This magnitude of growth will require concerted global efforts in every facet of PEMWE deployment—from fundamental research and component improvements to business strategies and federal policies. This section will provide a roadmap for the path forward.
7.1. Technical Targets
Overall PEMWE technical targets are proposed in Table 4. These values are based on a compilation of reports from numerous agencies and academic papers from across the globe, with representation from North America (U.S. DOE),242 South America,471 Africa,472 Asia,9,47,474 Europe (E.U. Clean Hydrogen Partnership),8,146,166,476,479 and international agencies (IRENA).141 Targets were corroborated by leading representatives in industry.
Table 4. Technical Targets for PEM Water Electrolysis.
| parameter | units | 2024 status | 2030 target | 2050 target | R&D focus | importance |
|---|---|---|---|---|---|---|
| System CapEx | $/kW | 1000 | 700 | 200 | BoP | Med |
| Stack CapEx | $/kW | 400 | 150 | 50 | MEA, PTL, BPP | High |
| H2 Production Cost | $/kg | 5 | 1.5 | 0.5 | MEA | High |
| Lifetime | 1000 h | 60 | 80 | 100 | MEA, PTL | Med |
| Degradation | %/1000 h | 25 | 15 | 10 | MEA, PTL | Med |
| System Efficiency | % LHV | 65 | 70 | 75 | BoP | Med |
| Stack Efficiency | % LHV | 70 | 75 | 80 | MEA | Med |
| Current Density (Nominal) | A·cm–2 | 2 | 3 | 5 | MEA, PTL | High |
| Voltage (Nominal) | V | 2 | 1.8 | 1.7 | PEM | Med |
| Anode Loading | mgIr·cm–2 | 1 | 0.4 | 0.1 | MEA, PTL | High |
| Cathode Loading | mgPt·cm–2 | 0.5 | 0.1 | 0.025 | MEA, GDL | Low |
| Membrane Thickness | μm | 150 | 80 | 50 | PEM | High |
| H2 Pressure | bar | <30 | 30 | 30 | PEM | Low |
7.1.1. Cost
System and stack CapEx greatly influence hydrogen production costs. At the system level (which comprises the stack and BoP), increasing manufacturing capabilities in production volume and unit size (from kW to GW capacities) will be the primary driver for cost reductions. Other drivers include improving equipment utilization, utilizing roll-to-roll assembly, and increasing automation. At the stack level, component costs dominate, particularly the MEA, PTL, and BPP. While increasing manufacturing volume will reduce costs, material costs will begin to dominate at higher volumes (Figure 7a). As the MEA can comprise nearly half of the stack cost at these scales, PGM loadings must be reduced while maintaining PEMWE activity and durability. Novel base materials and coatings for BPPs and PTLs, which are currently made of titanium and platinum, also need to be developed. Stainless steel is a promising base material for both.
Lastly, hydrogen production costs will highly depend on electricity prices and capacity factors (Figure 4). Load-following for cheap renewable electricity will be critical. Operating at high capacity factors will reduce costs substantially, but periods of low load are inevitable. Thus, grid control algorithms and management strategies are required.
7.1.2. Durability
Commercial systems use high PGM loadings for MEAs, PTLs, and BPPs to ensure adequate durability, leading to prohibitively high costs for large-scale deployment. Thus, developing cost-effective components that can reach lifetime targets will be a primary research focus. Optimizing the CL-PTL interface will be imperative to mitigate degradation, especially at low loadings; incorporating an MPL on the PTL surface is a promising strategy. Also, membrane durability will become increasingly relevant as thinner membranes are implemented. Reinforcements, recombinant catalysts, and radical scavengers can be incorporated to combat any increased susceptibility to mechanical and chemical damage. Lastly, cell components are currently optimized for constant-load operation, but PEMWEs will likely need to operate dynamically for load following. Thus, degradation under such conditions must be thoroughly assessed during durability testing.
Standardized ASTs are required to ensure objective comparison between data sets and to assess durability under industrially relevant conditions (i.e., load following). While no such tests are currently established, ASTs for each PEMWE cell component have been proposed in Table 3.
7.1.3. Efficiency
Achieving targets for stack efficiency (80% LHV) and nominal operating conditions (5 A·cm–2 at 1.7 V) will rely on improvements in the membrane, anode CL, and PTL. Developing highly active low-loading anode CLs will require creating homogeneous, electronically connected networks. Utilizing TiO2 supports can help, but the challenge of forming percolating IrOx networks needs to be overcome. Optimizing PTL properties—such as porosity and pore size—can reduce mass transport losses and increase catalyst utilization. Incorporating an MPL can also increase utilization by enhancing CL-PTL interfacial contact. Lastly, reductions in membrane thickness will be imperative due to decreased ohmic overpotentials, but care must be taken to limit degradation and gas crossover.
7.2. Manufacturability
Given the current deployment of PEMWEs, considerations for large-scale manufacturing have largely been overlooked in the literature. Thus, issues will arise when standard lab-scale fabrication techniques cannot be employed at high throughput. For example, most of the high-performing low-loading CLs in the literature were created using spray coating,137,175,481 which is less suitable for roll-to-roll manufacturing than methods involving sweeping a tool over a substrate (e.g., slot-die coating, gravure coating, and screen printing). Furthermore, since optimal ink composition varies between methods, transferring knowledge acquired from one method to another can be ineffective. The authors recommend that more focus be put on fabrication techniques that are more suitable for large-scale production. In addition, the PTL fabrication process must also be improved for reliable high-throughput manufacturing. In-line quality controls will be necessary to detect surface defects, impurities, edge warps, and inhomogeneities. Without stringent efforts to guarantee CL and PTL quality, stack-level failures can occur and impart significant setbacks to large-scale operations.
7.3. Policies
The number of countries implementing green hydrogen policies is growing rapidly, with ∼50 countries to date. This trajectory must be continued to meet deployment targets. However, despite the ambitious policies presented, a vast discrepancy exists between active projects and projects in the early planning stages. Projects that are active or up to final investment decision (FID) constitute only 7% of total announced projects, amounting to a mere 0.7 GW of PEMWE deployment. Given that 220 GW are required by 2030 to reach net zero emissions, policymakers must substantially accelerate green hydrogen projects.
8. Conclusion
The vast global participation for PEMWEs provides much confidence for the future. With concerted efforts in every developmental facet, the path to GW-scale deployment can be realized. Fundamental research for improving activity and durability while limiting costs is necessary. Large-scale manufacturability must be considered in conjunction with component developments. As technological readiness levels increase, a mature set of codes and standards must be established to ensure safe operation. Lastly, global green hydrogen policies must be monitored to ensure that targets are reached. This review has captured the current state of PEMWEs and provided an overarching roadmap for gigawatt-scale deployment.
Acknowledgments
The authors acknowledge the Department of Energy–Office of Energy Efficiency and Renewable Energy–Fuel Cell Technologies Office (DOE-EERE-FCTO) and the H2 from the Next-generation of Electrolyzers of Water (H2NEW) consortium for funding (and contract number DE-AC02-05CH11231 for J.K.L. and X.P.). D.K. was supported by U.S. Department of Energy award number DE-EE0009238. A.M.P. was supported by Department of Energy Grant DE-EE0008836. C.P.L. was supported by the National Science Foundation Graduate Research Fellowship Program under Grant No. DGE-1839285. Any opinions, findings, or conclusions or recommendations expressed in this material are those of the authors and do not necessarily reflect the views of the National Science Foundation.
Biographies
Cliffton Ray Wang received his B.A. from Harvard University in 2021 where he wrote his undergraduate thesis on modeling electrolyte conductivity in aqueous organic redox flow batteries under the guidance of Professor Michael J. Aziz. He is currently pursuing a Ph.D. in Chemical Engineering from the University of California, Irvine under Professor Iryna V. Zenyuk. His work focuses on determining structure–function relationships for iridium oxide catalysts in proton exchange membrane water electrolyzers.
John M. Stansberry is a Senior Scientist at the National Fuel Cell Research Center of the Clean Energy Institute at University of California, Irvine, as well as Senior Technical Program Manager at KRE Consulting LLC. He received his Ph.D. in Mechanical and Aerospace Engineering from University of California, Irvine in 2024. He has participated in a number of hydrogen-based energy conversion projects, including leading the UCI power-to-gas demonstration in the U.S. first injection of hydrogen into a working natural gas pipeline, consulting on the SoCalGas H2 Home project, and focusing his doctoral studies on the separation of hydrogen gas using electrochemical hydrogen pump cells. Currently, his work focuses on the optimization of the membrane electrode assembly for high-temperature proton exchange membrane-based cells and alternative renewable hydrogen-based fuels for solid oxide fuel cells.
Rangachary Mukundan (Mukund) is a Senior Scientist in the Energy Technologies Area at the Lawrence Berkeley National Laboratory (LBNL). His research interests include fuel cells, electrolyzers, flow batteries, and sensors. He is serving as deputy director in DOE’s Million Mile Fuel Cell Truck (M2FCT) and H2 from the Next-generation of Electrolyzers of Water (H2NEW). His primary research focus in these consortia is durability and development of accelerated stress tests. Mukund received his Ph.D. in Materials Science and Engineering from the University of Pennsylvania (Philadelphia) in February 1997. His work has been recognized through numerous awards, including two R&D 100 awards (1999, 2017), the Scientific American’s top 50 Science and Technology achievements for 2003, the J.B Wagner Award of the High Temperature Materials Division of the Electrochemical Society in 2005, and the Sensor Division outstanding achievement award in 2016. He is a fellow of the ECS and AAAS.
Hung-Ming Joseph Chang was born in Taiwan. He received his M.S. in Polymer Science and Engineering from the National Taiwan University, Taiwan and received a B.S. in Chemical and Materials Engineering from Chang Gung University, Taiwan. He joined the University of California, Irvine to pursue a Ph.D. degree in Chemical and Biomolecular Engineering in 2020. He is currently working in Professor Iryna Zenyuk’s group as a Ph.D. candidate. His work focuses on low-loading-supported IrOx catalysts in proton exchange membrane water electrolyzers (PEMWEs), operando X-ray micro-CT of PEMWEs, electrochemical CO2 reduction reaction, and cement precursor production via electrochemical processes.
Devashish Kulkarni is an R&D Engineer at Nel Hydrogen US. He earned his B.E. in Mechanical Engineering from the Maharashtra Institute of Technology in 2018 and completed his Ph.D. in Materials Science and Engineering from the University of California, Irvine in 2022 under the guidance of Prof. Iryna Zenyuk. During his graduate studies, he focused on optimizing interfaces and understanding transport processes to enable low catalyst loadings in polymer electrolyte membrane (PEM) electrolyzers. Currently, his primary focus is on cell stack design and deployment of MW-scale PEM electrolyzers. Additionally, he also serves as a technical team lead on various US Department of Energy projects for PEM electrolysis and fuel cells.
Andrew M. Park is a Senior Principal Engineer with The Chemours Company. He has >15 years’ experience in the manufacture and evaluation of membranes and membrane electrode assemblies for hydrogen fuel cells and water electrolyzers. Currently, Andrew leads efforts in Nafion membrane and ionomer research and development at Chemours. He received a Ph.D. from Vanderbilt University in Chemical and Biomolecular Engineering and a B.S. in Biosystems Engineering from Clemson University.
Austin B. Plymill is a Senior Staff Scientist at The Chemours Company leading research and technology development for Nafion products implemented in hydrogen-based technologies. Here, Austin leads research on membrane electrode assembly integration of ionomer components. Austin received a Ph.D. in Materials Science and Engineering from Northwestern University and received a B.S. in Materials Science and Engineering from The University of Tennessee, Knoxville.
Nausir Mahmoud Firas received his B.S. in Mechanical Engineering with a specialization in Energy Systems and Environmental Engineering and his M.S. in Mechanical and Aerospace Engineering from the University of California, Irvine (UCI) in 2021 and 2024, respectively. He is currently pursuing his Ph.D. at UCI under Professor Iryna Zenyuk. His work is focused on modeling performance impacts of flow fields and porous transport layers on proton exchange membrane water electrolyzers.
Christopher Pantayatiwong Liu is a Ph.D. student and National Science Foundation Graduate Research Fellow advised by Professor Plamen Atanassov. His research investigates the activity and degradation mechanisms of oxygen evolution catalysts in both acidic and alkaline systems. He holds a B.S. in Chemical Engineering from the University of California, Irvine (UCI, 2022), where he investigated the wettability of gas diffusion layers for proton exchange membrane fuel cell water management under the supervision of Professor Iryna Zenyuk. He is also the President of the ECS Student Chapter at UCI (ECS@UCI).
Jack T. Lang received his B.S. in Chemical Engineering from the University of California, Irvine (UCI) in 2022. He was an undergraduate researcher in Professor Iryna Zenyuk’s group where he performed rotating disk electrode experiments and X-ray CT image analysis. Currently, he is pursuing his Ph.D. at UCI in Professor Iryna Zenyuk’s group. His work now focuses on operando and ex situ X-ray CT imaging of transport layers for electrochemical cells and continuum modeling for water electrolysis.
Jason Keonhag Lee serves as an Assistant Professor in the Department of Mechanical Engineering at the University of Victoria. His research focuses on advancing clean hydrogen production technologies through electrochemical energy conversion. He earned his Ph.D. from the Department of Mechanical and Industrial Engineering at the University of Toronto and obtained his M.A.Sc. and B.Eng. from the Department of Mechanical Engineering at the University of Victoria. Dr. Lee worked as a postdoctoral researcher at Lawrence Berkeley National Laboratory where he contributed to the development of electrolyzers for reducing the cost of clean hydrogen.
Nadia E. Tolouei is a Ph.D. student at University of California, Irvine in the Chemical Engineering department in Professor Iryna Zenyuk’s group. She received her master’s degree in mechanical engineering at Southern Illinois university focusing on microelectromechanical systems. She has experience in fuel cell three-phase modeling. Her work now focuses on PEM water electrolyzer durability and investigating the in-plane movement of iridium catalyst throughout the MEA.
Yu Morimoto is a Chief Scientist at the National Fuel Cell Research Center of the University of California, Irvine (UCI). Before joining UCI in 2022, he was a research engineer in Toyota Central R&D Laboratories, Inc. in Nagoya, Japan, for more than 30 years focusing mainly on electrochemical devices and has contributed to the fuel cell systems for FCV Mirai. He received a Ph.D. from Case Western Reserve University and a B.S. and M.S. from Nagoya University.
CH Wang is the cofounder and CTO of TreadStone. He has led the technology development and commercialization of the corrosion-resistant metal plate technology for fuel cell, battery, and electrolyzer applications in last 10 years. Dr. Wang has extensive experience in electrochemistry devices, advanced materials design and processing, corrosion protection, and thin film materials and has contributed his experiences in a variety of energy-related technology developments, including PEM fuel cells, electrolyzers, solid oxide fuel cells, batteries, and gas separation membranes. Before starting TreadStone, Dr. Wang worked at Sarnoff Corporation as the technical leader in fuel cell technology development. Before joining Sarnoff, he worked at University of Pennsylvania as a research associate. Dr. Wang received his Ph.D. degree in Physical Chemistry from University of Science and Technology, Beijing, China. Dr. Wang is a member of American Electrochemical Society, and has over 20 publications and 10 US patents and patent applications.
Gaohua Zhu is a Principal Scientist at Toyota Research Institute of North America (TRINA) where he serves as the technical leader for fuel cells and water electrolyzers. He received his Ph.D. in Physics from Boston College and a B.S. in Materials Physics from Nanjing University, China. His research focuses on electrochemical energy conversion materials and processes, nanoengineered surfaces and materials, and thermal transport at nanoscale.
Jack Brouwer is Professor and Chancellor’s Fellow in Mechanical and Aerospace Engineering, Civil and Environmental Engineering, and Chemical and Biomolecular Engineering, and Director of the Clean Energy Institute (https://www.cleanenergy.uci.edu/) at the University of California, Irvine. Professor Brouwer is an energy system dynamics expert with research interests in renewable energy systems; dynamic simulation and control; energy system thermodynamics, design, and integration; electrochemical conversion devices and systems such as fuel cells, electrolyzers, and batteries; hydrogen production, storage, and conversion systems; hydrogen transmission, distribution, and dispensing; and electrochemical reactions with concurrent heat, mass, and momentum transfer. Professor Brouwer obtained his M.S. and B.S. in Mechanical Engineering from UCI and his Ph.D. in Mechanical Engineering and Post-Doc in Chemical Engineering at MIT.
Plamen Atanassov is a Chancellor’s Professor of Chemical & Biomolecular Engineering, University of California, Irvine where his research focuses on development of nonplatinum electrocatalysts, nanostructured platinum-based catalysts and advanced supports for fuel cells and electrolyzers, catalysts for CO2 electroreduction and products valorization, ammonia and urea electrosynthesis, and other new materials and technologies for energy conversion and storage. He is a senior advisor for business development to California’s DOE hydrogen hub–the Alliance for Renewable Clean Hydrogen Energy Systems (ARCHES) and interfacing with hydrogen technology demonstration and research efforts regionally and nationwide. Plamen Atanassov was inducted into the National Academy of Inventors and he is a Fellow of both The Electrochemical Society and the International Society of Electrochemistry for which he is the current President-elect.
Christopher B. Capuano is currently Director of CR&D Programs and has led numerous IR&D-funded cell design projects, as well as externally funded contracts through NSF, ONR, DOE, ARPAe, and NYSERDA. He is currently leading Nel’s joint development effort with General Motors to design and launch their next-generation cell stack, as well as the testing infrastructure required to support it. Mr. Capuano recently led the successful deployment of one of Europe’s largest PEM electrolyzers through concept phase to commissioning with the installation of a 20 MW plant used to support green ammonia synthesis.
Cortney Mittelsteadt (“Corky”) is currently the Vice President of Electrolyzer Technology for Plug Power. He established and is GM of Plug’s new manufacturing, R&D and sales center in Concord, MA. He is responsible for technical direction on electrolyzer stack technology to improve performance while dropping costs through technology, manufacturing, and supply chain improvements. Prior to that, Corky was at Giner, Inc. for 21 years, the last three as CEO, where he led negotiations with Plug Power to acquire Giner ELX. He oversaw the cooperation between Giner/General Motors to develop high-temperature fuel cells for automotive use. Dr. Mittelsteadt received his B.S. in Chemical Engineering from Rose-Hulman, his Ph.D. in Chemistry from SUNY-ESF/Syracuse University, and his MBA from MIT.
Xiong Peng is a scientist at Lawrence Berkeley National Laboratory. His research focuses on addressing critical performance and durability challenges in membrane-based water electrolysis devices for green hydrogen production.
Iryna V. Zenyuk is a Professor in the Department of Chemical and Biomolecular Engineering. Zenyuk holds a B.S. (2008) in mechanical engineering from the New York University Tandon School of Engineering. She continued her studies at Carnegie Mellon University where she earned an M.S. (2011) and Ph.D. (2013) in mechanical engineering. Zenyuk did her postdoctoral fellowship at Lawrence Berkeley National Laboratory in Electrochemical Technologies Group. Prof. Zenyuk has published over 100 journal publications and delivered more than 150 invited presentations on topics of energy conversion and storage.
Author Contributions
CRediT: Cliffton Ray Wang conceptualization, data curation, formal analysis, investigation, methodology, software, visualization, writing - original draft, writing - review & editing; John M. Stansberry data curation, formal analysis, methodology, visualization, writing - original draft, writing - review & editing; Rangachary Mukundan funding acquisition, investigation, methodology, writing - original draft, writing - review & editing; Hung-Ming Joseph Chang software, visualization, writing - review & editing; Devashish Kulkarni formal analysis, methodology, software, writing - original draft, writing - review & editing; Andrew M. Park supervision, writing - original draft, writing - review & editing; Austin B. Plymill writing - original draft, writing - review & editing; Nausir Mahmoud Firas formal analysis, investigation, methodology, software, visualization, writing - original draft; Christopher Pantayatiwong Liu formal analysis, writing - original draft, writing - review & editing; Jack T. Lang formal analysis, methodology, visualization, writing - original draft, writing - review & editing; Jason Keonhag Lee data curation, methodology, writing - original draft, writing - review & editing; Nadia E. Tolouei visualization, writing - original draft; Yu Morimoto investigation, supervision; CH Wang writing - original draft, writing - review & editing; Gaohua Zhu methodology, writing - original draft, writing - review & editing; Jack Brouwer supervision, writing - original draft, writing - review & editing; Plamen Atanassov investigation, supervision; Christopher B. Capuano investigation, methodology, writing - original draft, writing - review & editing; Xiong Peng funding acquisition, supervision, writing - original draft, writing - review & editing; Cortney Mittelsteadt investigation, methodology, writing - original draft, writing - review & editing; Iryna V. Zenyuk conceptualization, funding acquisition, resources, supervision, writing - review & editing.
The authors declare no competing financial interest.
Special Issue
Published as part of Chemical Reviewsspecial issue “Green Hydrogen”.
References
- Pellow M. A.; Emmott C. J. M.; Barnhart C. J.; Benson S. M. Hydrogen or Batteries for Grid Storage? A Net Energy Analysis. Energy Environ. Sci. 2015, 8 (7), 1938–1952. 10.1039/C4EE04041D. [DOI] [Google Scholar]
- Pivovar B.; Rustagi N.; Satyapal S. Hydrogen at Scale (H2@Scale): Key to a Clean, Economic, and Sustainable Energy System. Electrochem Soc. Interface 2018, 27 (1), 47. 10.1149/2.F04181if. [DOI] [Google Scholar]
- Aslam S.; Rani S.; Lal K.; Fatima M.; Hardwick T.; Shirinfar B.; Ahmed N. Electrochemical Hydrogen Production: Sustainable Hydrogen Economy. Green Chemistry. 2023, 25, 9543–9573. 10.1039/D3GC02849F. [DOI] [Google Scholar]
- Clapp M.; Zalitis C. M.; Ryan M. Perspectives on Current and Future Iridium Demand and Iridium Oxide Catalysts for PEM Water Electrolysis. Catal. Today 2023, 420 (March), 114140. 10.1016/j.cattod.2023.114140. [DOI] [Google Scholar]
- International Energy Agency . Global Hydrogen Review 2022, IEA, Paris; 2022. www.iea.org/t&c/. [Google Scholar]
- US Department of Energy . Fact of the month august 2018: Global electrolyzer sales reach 100 MW per year. [Google Scholar]
- International Energy Agency . Tracking Clean Energy Progress 2023, IEA, Paris; 2023. [Google Scholar]
- Carmo M.; Fritz D. L.; Mergel J.; Stolten D. A Comprehensive Review on PEM Water Electrolysis. International Journal of Hydrogen Energy. 2013, 38 ((12)), 4901–4934. 10.1016/j.ijhydene.2013.01.151. [DOI] [Google Scholar]
- Shiva Kumar S.; Himabindu V. Hydrogen Production by PEM Water Electrolysis - A Review. Mater. Sci. Energy Technol. 2019, 2, 442–454. 10.1016/j.mset.2019.03.002. [DOI] [Google Scholar]
- Pandiyan A.; Uthayakumar A.; Subrayan R.; Cha S. W.; Krishna Moorthy S. B. Review of Solid Oxide Electrolysis Cells: A Clean Energy Strategy for Hydrogen Generation. Nanomaterials and Energy 2019, 8 (1), 2–22. 10.1680/jnaen.18.00009. [DOI] [Google Scholar]
- Rashid M.; Khaloofah M.; Mesfer A.; Naseem H.; Danish M.; Al Mesfer M. K. Hydrogen Production by Water Electrolysis: A Review of Alkaline Water Electrolysis, PEM Water Electrolysis and High Temperature Water Electrolysis. International Journal of Engineering and Advanced Technology 2015, 4 (3), 80–93. [Google Scholar]
- Brauns J.; Turek T. Alkaline Water Electrolysis Powered by Renewable Energy: A Review. Processes 2020, 8 (2), 248. 10.3390/pr8020248. [DOI] [Google Scholar]
- Villagra A.; Millet P. An Analysis of PEM Water Electrolysis Cells Operating at Elevated Current Densities. Int. J. Hydrogen Energy 2019, 44 (20), 9708–9717. 10.1016/j.ijhydene.2018.11.179. [DOI] [Google Scholar]
- Lewinski K. A.; Luopa S. M.; Sun F.; Jentzsch C.; van der Vliet D. F. (Invited) High Power Water Electrolysis as a New Paradigm for Operation of PEM Electrolyzer - The Story Continues. ECS Meeting Abstracts 2018, MA2018-01 (29), 1637. 10.1149/MA2018-01/29/1637. [DOI] [Google Scholar]
- Shin H.-S.; Oh B. S. Water Transport According to Temperature and Current in PEM Water Electrolyzer. Int. J. Hydrogen Energy 2020, 45 (1), 56–63. 10.1016/j.ijhydene.2019.10.209. [DOI] [Google Scholar]
- Ni M.; Leung M. K. H.; Leung D. Y. C. Energy and Exergy Analysis of Hydrogen Production by a Proton Exchange Membrane (PEM) Electrolyzer Plant. Energy Convers Manag 2008, 49 (10), 2748–2756. 10.1016/j.enconman.2008.03.018. [DOI] [Google Scholar]
- Luo X.; Lau G.; Tesfaye M.; Arthurs C. R.; Cordova I.; Wang C.; Yandrasits M.; Kusoglu A. Thickness Dependence of Proton-Exchange-Membrane Properties. J. Electrochem. Soc. 2021, 168 (10), 104517. 10.1149/1945-7111/ac2973. [DOI] [Google Scholar]
- Pham C.; Escalera López D.; Mayrhofer K.; Cherevko S.; Thiele S. Essentials of High Performance Water Electrolyzers - From Catalyst Layer Materials to Electrode Engineering. Adv. Energy Mater. 2021, 11, 2101998. 10.1002/aenm.202101998. [DOI] [Google Scholar]
- Pollet B. G.; Franco A. A.; Su H.; Liang H.; Pasupathi S.. 1 - Proton Exchange Membrane Fuel Cells. In Compendium of Hydrogen Energy; Barbir F.; Basile A.; Veziroğlu T. N., Eds.; Woodhead Publishing: Oxford, 2016; pp 3–56. [Google Scholar]
- Parra-Restrepo J.; Bligny R.; Dillet J.; Didierjean S.; Stemmelen D.; Moyne C.; Degiovanni A.; Maranzana G. Influence of the Porous Transport Layer Properties on the Mass and Charge Transfer in a Segmented PEM Electrolyzer. Int. J. Hydrogen Energy 2020, 45 (15), 8094–8106. 10.1016/j.ijhydene.2020.01.100. [DOI] [Google Scholar]
- Badgett A.; Brauch J.; Thatte A.; Rubin R.; Skangos C.; Wang X.; Ahluwalia R.; Pivovar B.; Ruth M.. Updated Manufactured Cost Analysis for Proton Exchange Membrane Water Electrolyzers; 2023. www.nrel.gov/publications.
- Park S.; Lee W.; Na Y. Performance Comparison of Proton Exchange Membrane Water Electrolysis Cell Using Channel and PTL Flow Fields through Three-Dimensional Two-Phase Flow Simulation. Membranes 2022, 12 (12), 1260. 10.3390/membranes12121260. [DOI] [PMC free article] [PubMed] [Google Scholar]
- Heraeus Precious Metals. Iridium and Platinum Catalysts for PEM Electrolyzers. https://www.heraeus.com/en/hpm/hmp_products_solutions/hydrogensystems/hydrogen_generation/hydrogen_generation.html?websiteCriteria=0010.
- Newtrace . The critical role of materials in the high price of PEM electrolyzers; 2022. hhttps://www.newtrace.io/post/the-critical-role-of-materials-in-the-high-price-of-pem-electrolyzers#:~:text=Furthermore%2C%20the%20cost%20of%20manufacturing,temperature%20electrolyzers%20such%20as%20AWE. [Google Scholar]
- Kato T.; Kubota M.; Kobayashi N.; Suzuoki Y. Effective Utilization of By-Product Oxygen from Electrolysis Hydrogen Production. Energy 2005, 30 (14), 2580–2595. 10.1016/j.energy.2004.07.004. [DOI] [Google Scholar]
- Sakurai M.; Shima A.; Terao T.. Study on Water Electrolysis for Oxygen Production-Reduction of Water Circulation and Gas-Liquid Separator. 47th International Conference on Environmental Systems, Charleston, SC, July 16–20, 2017.
- Giddey S.; Ciacchi F. T.; Badwal S. P. S. High Purity Oxygen Production with a Polymer Electrolyte Membrane Electrolyser. J. Membr. Sci. 2010, 346 (1), 227–232. 10.1016/j.memsci.2009.09.042. [DOI] [Google Scholar]
- Medina P.; Santarelli M. Analysis of Water Transport in a High Pressure PEM Electrolyzer. Int. J. Hydrogen Energy 2010, 35 (11), 5173–5186. 10.1016/j.ijhydene.2010.02.130. [DOI] [Google Scholar]
- Liu Y.; Amin Md. T.; Khan F.; Pistikopoulos E. N. Safety Analysis of Proton Exchange Membrane Water Electrolysis System. J. Environ. Chem. Eng. 2023, 11 (5), 110772. 10.1016/j.jece.2023.110772. [DOI] [Google Scholar]
- Kai J.; Saito R.; Terabaru K.; Li H.; Nakajima H.; Ito K. Effect of Temperature on the Performance of Polymer Electrolyte Membrane Water Electrolysis: Numerical Analysis of Electrolysis Voltage Considering Gas/Liquid Two-Phase Flow. J. Electrochem. Soc. 2019, 166 (4), F246–F254. 10.1149/2.0521904jes. [DOI] [Google Scholar]
- Xu W.; Scott K.; Basu S. Performance of a High Temperature Polymer Electrolyte Membrane Water Electrolyser. J. Power Sources 2011, 196, 8918–8924. 10.1016/j.jpowsour.2010.12.039. [DOI] [Google Scholar]
- Hancke R.; Holm T.; Ulleberg Ø. The Case for High-Pressure PEM Water Electrolysis. Energy Convers. Manage. 2022, 261, 115642. 10.1016/j.enconman.2022.115642. [DOI] [Google Scholar]
- Hancke R.; Bujlo P.; Ulleberg Ø. Design and Testing of a High-Pressure PEM Water Electrolyzer System Test Rig. ECS Meeting Abstracts 2021, MA2021-02, 1244. 10.1149/MA2021-02411244mtgabs. [DOI] [Google Scholar]
- Aili D.; Hansen M. K.; Pan C.; Li Q.; Christensen E.; Jensen J. O.; Bjerrum N. J. Phosphoric Acid Doped Membranes Based on Nafion®, PBI and Their Blends - Membrane Preparation, Characterization and Steam Electrolysis Testing. Int. J. Hydrogen Energy 2011, 36 (12), 6985–6993. 10.1016/j.ijhydene.2011.03.058. [DOI] [Google Scholar]
- Antonucci V.; Di Blasi A.; Baglio V.; Ornelas R.; Matteucci F.; Ledesma-Garcia J.; Arriaga L. G.; Aricò A. S. High Temperature Operation of a Composite Membrane-Based Solid Polymer Electrolyte Water Electrolyser. Electrochim. Acta 2008, 53 (24), 7350–7356. 10.1016/j.electacta.2008.04.009. [DOI] [Google Scholar]
- Antonucci P. L.; Aricò A. S.; Cretı P.; Ramunni E.; Antonucci V. Investigation of a Direct Methanol Fuel Cell Based on a Composite Nafion®-Silica Electrolyte for High Temperature Operation. Solid State Ion 1999, 125 (1), 431–437. 10.1016/S0167-2738(99)00206-4. [DOI] [Google Scholar]
- Watanabe M.; Uchida H.; Seki Y.; Emori M.; Stonehart P. Self-Humidifying Polymer Electrolyte Membranes for Fuel Cells. J. Electrochem. Soc. 1996, 143, 3847. 10.1149/1.1837307. [DOI] [Google Scholar]
- Alberti G.; Casciola M. Composite Membranes for Medium-Temperature PEM Fuel Cells. Annual Review of Materials Research - ANNU REV MATER RES 2003, 33, 129–154. 10.1146/annurev.matsci.33.022702.154702. [DOI] [Google Scholar]
- Costamagna P.; Yang C.; Bocarsly A. B.; Srinivasan S. Nafion® 115/Zirconium Phosphate Composite Membranes for Operation of PEMFCs above 100°C. Electrochim. Acta 2002, 47 (7), 1023–1033. 10.1016/S0013-4686(01)00829-5. [DOI] [Google Scholar]
- Alberti G.; Casciola M.; Pica M.; Tarpanelli T.; Sganappa M. New Preparation Methods for Composite Membranes for Medium Temperature Fuel Cells Based on Precursor Solutions of Insoluble Inorganic Compounds. Fuel Cells 2005, 5 (3), 366–374. 10.1002/fuce.200400070. [DOI] [Google Scholar]
- Grigoriev S. A.; Millet P.; Korobtsev S. V.; Porembskiy V. I.; Pepic M.; Etievant C.; Puyenchet C.; Fateev V. N. Hydrogen Safety Aspects Related to High-Pressure Polymer Electrolyte Membrane Water Electrolysis. Int. J. Hydrogen Energy 2009, 34 (14), 5986–5991. 10.1016/j.ijhydene.2009.01.047. [DOI] [Google Scholar]
- Hystar . Patented Technology. https://hystar.com/pem/. [Google Scholar]
- Zhang K.; Liang X.; Wang L.; Sun K.; Wang Y.; Xie Z.; Wu Q.; Bai X.; Hamdy M. S.; Chen H.; Zou X. Status and Perspectives of Key Materials for PEM Electrolyzer. Nano Research Energy 2022, 1 (3), 9120032. 10.26599/NRE.2022.9120032. [DOI] [Google Scholar]
- Liu R.-T.; XU Z.-L.; Li F.-M.; Chen F.-Y.; Yu J.-Y.; Yan Y.; Chen Y.; Xia B. Y. Recent Advances in Proton Exchange Membrane Water Electrolysis. Chem. Soc. Rev. 2023, 52, 5652. 10.1039/D2CS00681B. [DOI] [PubMed] [Google Scholar]
- Wang T.; Cao X.; Jiao L. PEM Water Electrolysis for Hydrogen Production: Fundamentals, Advances, and Prospects. Carbon Neutrality 2022, 1, 21. 10.1007/s43979-022-00022-8. [DOI] [Google Scholar]
- Feng Q.; Yuan X.; Liu G.; Wei B.; Zhang Z.; Li H.; Wang H. A Review of Proton Exchange Membrane Water Electrolysis on Degradation Mechanisms and Mitigation Strategies. J. Power Sources 2017, 366, 33–55. 10.1016/j.jpowsour.2017.09.006. [DOI] [Google Scholar]
- International Energy Agency . Global Hydrogen Review 2021; IEA: Paris, 2021. https://www.iea.org/reports/global-hydrogen-review-2021. [Google Scholar]
- Plug Power, Inc.. Plug 1MW Electrolyzer Commissioned at World’s First Floating Offshore Green Hydrogen Production Site; 2022. https://www.ir.plugpower.com/press-releases/news-details/2022/Plug-1MW-Electrolyzer-Commissioned-at-Worlds-First-Floating-Offshore-Green-Hydrogen-Production-Site/default.aspx.
- H2 International. WindGas Project in Hamburg-Reitbrook in Operation; 2016. https://h2-international.com/2016/02/04/windgas-project-in-hamburg-reitbrook-in-operation/#:~:text=Hamburg-Reitbrook%20is%20home%20to,of%20an%20NIP%20subsidy%20project.
- International Energy Agency . Global Hydrogen Review 2023; IEA: Paris, 2023. https://www.iea.org/reports/global-hydrogen-review-2023.
- Wappler M.; Unguder D.; Lu X.; Ohlmeyer H.; Teschke H.; Lueke W. Building the Green Hydrogen Market - Current State and Outlook on Green Hydrogen Demand and Electrolyzer Manufacturing. Int. J. Hydrogen Energy 2022, 47 (79), 33551–33570. 10.1016/j.ijhydene.2022.07.253. [DOI] [Google Scholar]
- CSIRO . HyResource International Policy. https://research.csiro.au/hyresource/policy/international/.
- Government of the Netherlands . Government Strategy on Hydrogen; 2020. https://www.government.nl/documents/publications/2020/04/06/government-strategy-on-hydrogen.
- Hydrogen and Fuel Cell Strategy Council . The Strategic Road Map for Hydrogen and Fuel Cells: Industry-Academia-Government Action Plan to Realize a Hydrogen Society; Japanese Ministry of Economy, Trade and Industry, 2019. http://www.meti.go.jp/press/2018/03/20190312001/20190312001-3.pdf [Google Scholar]
- Direção-Geral de Energia e Geologia . EN-H2 Estrategia Nacional Para o Hidrogenio (Vers Ao Draft) (Portugal); 2020. [Google Scholar]
- Ministry of Trade Industry and Energy (MOTIE) . Hydrogen Economy: Roadmap of Korea; 2019. [Google Scholar]
- Germany Federal Ministry for Economic Affairs and Energy . The National Hydrogen Strategy (Germany); 2020. [Google Scholar]
- Reuters . China sets green hydrogen target for 2025, eyes widespread use; 2022. https://www.reuters.com/world/china/china-produce-100000-200000-t-green-hydrogen-annually-by-2025-2022-03-23/.
- The Norwegian Government . Norwegian Government’s Hydrogen Strategy towards a Low Emission Society; 2020.
- Ministry of Trade and Industry . Singapore’s National Hydrogen Strategy. https://www.mti.gov.sg/Industries/Hydrogen (accessed 2024-09-18).
- Fuel Cells and Hydrogen Joint Undertaking . Hydrogen Roadmap Europe: A Sustainable Pathway for the European Energy Transition; 2019. 10.2843/249013. [DOI] [Google Scholar]
- Ministry of New and Renewable Energy . National Green Hydrogen Mission; Government of India, 2023. [Google Scholar]
- Ministry for the Ecological Transition . National Strategy for the Development of Decarbonised and Renewable Hydrogen in France; 2020. [Google Scholar]
- PSASL . Sri Lanka National Hydrogen Roadmap; 2023. https://api.greenstat.no/uploads/Sri_Lanka_Roadmap_Final_5b7d4aff51.pdf?updated_at=2023-08-02T14:11:03.276Z (accessed 2024-09-18).
- Ministerio para la Transición Ecológica y el Reto . Hydrogen Roadmap e a Commitment to Renewable Hydrogen - Executive Summary (Spain); 2020. [Google Scholar]
- MOSTI . Hydrogen Economy & Technology Roadmap. https://www.mosti.gov.my/en/dasar/#flipbook-df_69947/7/ (accessed 2024-09-18). [Google Scholar]
- Wiśniewska I.Concept for the development of hydrogen energy in Russia; Centre for Eastern Studies, 2021. https://www.osw.waw.pl/en/publikacje/analyses/2021-08-13/concept-development-hydrogen-energy-russia (accessed 2023-07-11).
- Saria L.. Indonesia’s National Hydrogen Strategy; Ministry of Energy and Mineral Resources, 2024. https://henca-tokyo.metro.tokyo.lg.jp/data/Ministry_of_Energy_and_Mineral_Resources_of_the_Republic_of_Indonesia.pdf (accessed 2024-09-18). [Google Scholar]
- Laurikko J.; Ihonen J.; Kiviaho J.; Himanen O.; Weiss R.; Saarinen V.; Kärki J.; Hurskainen M.. National Hydrogen Roadmap for Finland; 2020. [Google Scholar]
- Italy Ministero dello Sviluppo Economico . Strategia Nazionale Idrogeno Linee Guida Preliminari (Italy). [Google Scholar]
- Correa A.; Barrria Q.; PB M.. National Green Hydrogen Strategy (Chile); 2020. 10.1787/f661a3f7-en [DOI] [Google Scholar]
- Ministry of Energy of Ukraine . Draft Roadmap for Production and Use of Hydrogen in Ukraine; 2021. [Google Scholar]
- US Department of Energy . Department of Energy Hydrogen Program Plan; U.S. Department of Energy, 2020; p 56. [Google Scholar]
- Hungarian Government . Hungary’s National Hydrogen Strategy: Strategy for the Introduction of Clean Hydrogen and Hydrogen Technologies To the Domestic Market and for Establishing Background Infrastructure for the Hydrogen Industry; 2021. [Google Scholar]
- National Resources Canada . HYDROGEN STRATEGY FOR CANADA; 2020. [Google Scholar]
- Ministry of Climate and Environment. Polish Hydrogen Strategy until 2030 with an Outlook until 2040: Summary; 2021; pp 1–6. [Google Scholar]
- Vice Ministry of Mines and Energy (VMME) . Towards the Green Hydrogen Roadmap in Paraguay; 2021. [Google Scholar]
- Karin S.; Lukáš O.. Ministry of Industry and Trade presents Czech Hydrogen Strategy; KPMG. https://danovky.cz/en/news/detail/893 (accessed 2023-06-21).
- Ministerio de Minas y Energía . Colombia’s Hydrogen Roadmap; 2021. [Google Scholar]
- Sinay J.; Weiterschütz J.; Jesný M.; Blaškovitš P.; Sulík R.. National Hydrogen Strategy: Ready for the Future; 2023. https://www.enviroportal.sk/energetika/dokumenty/narodna-vodikova-strategia-pripraveni-na-buducnost-2021 (accessed 2024-09-18).
- Ministerio de Industria Energía y Minería . Green Hydrogen Roadmap in Uruguay; 2022. [Google Scholar]
- His Majesty’s Government (United Kingdom) . UK Hydrogen Strategy; 2021. 10.1002/cind.859_6.x. [DOI] [Google Scholar]
- Estrategia Nacional de Hidrógeno Verde (ENHIVE). https://www.energia.gob.pa/mdocs-posts/estrategia-nacional-de-hidrogeno-verde-enhive/ (accessed 2024-09-18).
- Jones J. S.Sweden - a national strategy for green hydrogen; Enlit, 2021. https://www.enlit.world/hydrogen/sweden-a-national-strategy-for-green-hydrogen/.
- Secretaría de Asuntos Estratégicos de la Presidencia de la Nación. Estrategia Nacional Para El Desarrollo de La Economía Del Hidrógeno; 2023. https://www.argentina.gob.ar/sites/default/files/2023/07/estrategia_nacional_de_hidrogeno_-_sae.pdf (accessed 2024-09-18).
- Danish Ministry of Climate Energy and Utilities . The Governments Strategy for Power-to-X; 2021. [Google Scholar]
- MINISTRY OF ECONOMY AND SUSTAINABLE DEVELOPMENT . HYDROGEN STRATEGY OF THE REPUBLIC OF CROATIA UNTIL 2050; 2022. [Google Scholar]
- Government of Morocco . Stategie Nationale de l’Hydrogene Vert; 2021. [Google Scholar]
- Federal Ministry Republic of Austria . Hydrogen Strategy for Austria - Executive Summary. 2022; pp 1–9. [Google Scholar]
- Republic of South Africa Department of Science & Innovation. Hydrogen Society Roadmap for South Africa 2021 Securing a Clean, Affordable and Sustainable Energy; 2021. [Google Scholar]
- Ministère belge de l’économie . Vision and Strategy - Hydrogen (Update October 2022); 2022.
- Green Hydrogen Organization . Namibia Green Hydrogen Vision. https://gh2.org/countries/namibia. [Google Scholar]
- Greek Hydrogen Strategy: Domestic production of 3,500 GWh in 2030. https://www.ot.gr/2022/06/07/english-edition/greek-hydrogen-strategy-domestic-production-of-3500-gwh-in-2030/.
- Ministry of Energy and Mines . Algerian National Hydrogen Development Strategy; 2023. [Google Scholar]
- Collins L.Algeria aims to supply Europe with 10% of its clean hydrogen needs by 2040 in new national H2 roadmap. HydrogenInsight, 2024. https://www.hydrogeninsight.com/policy/algeria-aims-to-supply-europe-with-10-of-its-clean-hydrogen-needs-by-2040-in-new-national-h2-roadmap/2-1-1426265?utm_source=email_campaign&utm_medium=email&utm_campaign=2023-03-30&utm_term=recharge&utm_content=hydrogen (accessed 2024-06-14).
- Le Gouvernement du Grand-duche de Luxembourg . Stratégie Hydrogène Du Luxembourg; 2021. [Google Scholar]
- Ministry of Energy and Petroleum . Green Hydrogen Strategy and Roadmap for Kenya; 2023. [Google Scholar]
- Romanian Ministry of Energy . Romanian National Hydrogen Strategy Project; 2023. https://energie.gov.ro/wp-content/uploads/2023/05/EN-Proiect-National-Hydrogen-Strategy.pdf (accessed 2024-09-18). [Google Scholar]
- Dokso A.Tunisia Aims to Produce 8.3 Million Tonnes of Green Hydrogen by 2050. https://energynews.biz/tunisia-aims-to-produce-8-3-million-tonnes-of-green-hydrogen-by-2050/ (accessed 2024-09-18).
- Department of the Environment, Climate and Communications . National Hydrogen Strategy Plan; Government of Ireland, 2023. [Google Scholar]
- Martin P.; Parkes R.. UAE targets 15 million tonnes of green hydrogen production by 2050 as it approves national H2 strategy; HydrogenInsight, 2023. https://www.hydrogeninsight.com/policy/uae-targets-15-million-tonnes-of-green-hydrogen-production-by-2050-as-it-approves-national-h2-strategy/2-1-1480383?utm_source=email_campaign&utm_medium=email&utm_campaign=2023-07-06&utm_term=recharge&utm_content=hydrogen (accessed 2023-07-09).
- Reuters . UAE targets 25% of global hydrogen fuel market by 2030. https://www.reuters.com/business/cop/uae-targets-25-global-hydrogen-fuel-market-by-2030-2021-11-04/ (accessed 2023-07-03). [Google Scholar]
- Ministry of Business Innovation & Employment . A Vision for Hydrogen in New Zealand: Green Paper; New Zealand Government, 2019. [Google Scholar]
- Oman News Agency . Agreements Worth Over RO 20 Billion for Green Hydrogen Projects in Oman Inked. https://omannews.gov.om/topics/en/80/show/112179. [Google Scholar]
- Foreign Ministry of Oman . Oman announces investment opportunities in green hydroge. https://fm.gov.om/oman-announces-investment-opportunities-in-green-hydrogen/. [Google Scholar]
- COAG Energy Council Hydrogen Working Group . National Hydrogen; 2019. [Google Scholar]
- Israel Ministry of Energy and Infrastructure . Israel Hydrogen Strategy - Guiding Principles and Decision Points; 2023. https://www.gov.il/BlobFolder/news/news-150523-2/en/israel-hydrogen-strategy-english.pdf (accessed 2024-09-18).
- Ministry of Energy and Natural Resources . Türkiye announces national energy plan and hydrogen strategy; Republic of Türkiye, 2023. https://enerji.gov.tr/news-detail?id=21111. [Google Scholar]
- The Oxford Institute for Energy Studies . Blue H2 as Enabler of Green: The Case of Germany; 2020. [Google Scholar]
- van Renssen S. The Hydrogen Solution?. Nat. Clim Chang 2020, 10 (9), 799–801. 10.1038/s41558-020-0891-0. [DOI] [Google Scholar]
- Dolci F.Green Hydrogen Opportunities in Selected Industrial Processes Workshop Summary Report; 2019. 10.2760/634063. [DOI] [Google Scholar]
- Australian Government . Guarantee of Origin. https://www.cleanenergyregulator.gov.au/Infohub/Markets/guarantee-of-origin (accessed 2023-07-12).
- Suleman F.; Dincer I.; Agelin-Chaab M. Environmental Impact Assessment and Comparison of Some Hydrogen Production Options. Int. J. Hydrogen Energy 2015, 40 (21), 6976–6987. 10.1016/j.ijhydene.2015.03.123. [DOI] [Google Scholar]
- Al-Qahtani A.; Parkinson B.; Hellgardt K.; Shah N.; Guillen-Gosalbez G. Uncovering the True Cost of Hydrogen Production Routes Using Life Cycle Monetisation. Appl. Energy 2021, 281, 115958. 10.1016/j.apenergy.2020.115958. [DOI] [Google Scholar]
- Mehmeti A.; Angelis-Dimakis A.; Arampatzis G.; McPhail S. J.; Ulgiati S. Life Cycle Assessment and Water Footprint of Hydrogen Production Methods: From Conventional to Emerging Technologies. Environments 2018, 5 (2), 24. 10.3390/environments5020024. [DOI] [Google Scholar]
- Salkuyeh Y. K.; Saville B. A.; MacLean H. L. Techno-Economic Analysis and Life Cycle Assessment of Hydrogen Production from Different Biomass Gasification Processes. Int. J. Hydrogen Energy 2018, 43 (20), 9514–9528. 10.1016/j.ijhydene.2018.04.024. [DOI] [Google Scholar]
- IEA . Hydrogen Projects Database. https://www.iea.org/data-and-statistics/data-product/hydrogen-production-and-infrastructure-projects-database#hydrogen-production-and-infrastructure-projects. [Google Scholar]
- Nadaleti W. C.; de Souza E. G.; Lourenço V. A. Green Hydrogen-Based Pathways and Alternatives: Towards the Renewable Energy Transition in South America’s Regions-Part B. Int. J. Hydrogen Energy 2022, 47 (1), 1–15. 10.1016/j.ijhydene.2021.05.113. [DOI] [Google Scholar]
- Kelman R.; Gaspar L. de S.; Geyer F. S.; Barroso L. A. N.; Pereira M. V. F. Can Brazil Become a Green Hydrogen Powerhouse?. Journal of Power and Energy Engineering 2020, 08 (11), 21–32. 10.4236/jpee.2020.811003. [DOI] [Google Scholar]
- Scatec . Scatec partners with Fertiglobe and the Sovereign Fund of Egypt to develop green hydrogen as feedstock for ammonia production in Egypt. https://scatec.com/2021/10/14/scatec-partners-with-fertiglobe-and-the-sovereign-fund-of-egypt-to-develop-green-hydrogen-as-feedstock-for-ammonia-production-in-egypt/ (accessed 2023-07-01).
- Angula V.. Namibia Signs $10 Billion Green Energy Deal With Germany’s Hyphen; Voice of America News, 2023. https://www.voanews.com/a/namibia-signs-10-billion-green-energy-deal-with-germany-s-hyphen-/7118163.html (accessed 2023-07-01).
- Gandhi K.; Apostoleris H.; Sgouridis S. Catching the Hydrogen Train: Economics-Driven Green Hydrogen Adoption Potential in the United Arab Emirates. Int. J. Hydrogen Energy 2022, 47 (53), 22285–22301. 10.1016/j.ijhydene.2022.05.055. [DOI] [Google Scholar]
- Ikken B.; Rachidi S.; Hirt A.; Nabil N.; Benmeziane M.. POWER-TO-X IN MOROCCO: Driver of Mediterranean Energy Market Integration; Research Institute for Solar Energy and New Energies, 2020. [Google Scholar]
- Menon A.Morocco’s First Green Hydrogen Project to Start Production in 2025; ZAWYA, 2021.https://www.zawya.com/en/business/moroccos-first-green-hydrogen-project-to-start-production-in-2025-ebtd9f4s.
- International Monetary Fund. Global Price of Natural Gas, EU [PNGASEUUSDM], Retrieved from FRED, Federal Reserve Bank of St. Louis. https://fred.stlouisfed.org/series/PNGASEUUSDM. [Google Scholar]
- Energy Institute . Statistical Review of World Energy, 73rd ed.; Energy Institute Statistical Review of World Energy, 2024. https://www.energyinst.org/statistical-review. [Google Scholar]
- Gonzales-Calienes G.; Kannangara M.; Shadbahr J.; Deces-Petit C.; Bensebaa F.; Mehr N. G.; Teguia C. D.; Akbari M.; Benali M.; Chen J.. Life Cycle Assessment of Hydrogen Production Pathways in Canada; National Research Council Canada, 2022. 10.4224/40002781. [DOI] [Google Scholar]
- Glenk G.; Reichelstein S. Economics of Converting Renewable Power to Hydrogen. Nat. Energy 2019, 4 (3), 216–222. 10.1038/s41560-019-0326-1. [DOI] [Google Scholar]
- Ayers K. High Efficiency PEM Water Electrolysis: Enabled by Advanced Catalysts, Membranes, and Processes. Curr. Opin Chem. Eng. 2021, 33, 100719. 10.1016/j.coche.2021.100719. [DOI] [Google Scholar]
- IEA . World Energy Outlook 2022 - Analysis; 2022. [Google Scholar]
- Ayers K. The Potential of Proton Exchange Membrane-Based Electrolysis Technology. Curr. Opin Electrochem 2019, 18, 9–15. 10.1016/j.coelec.2019.08.008. [DOI] [Google Scholar]
- Peterson D.; Vickers J.; Desantis D.. Hydrogen Production Cost From PEM Electrolysis - 2019; Department of Energy, 2020. http://www.hydrogen.energy.gov/h2a_prod_studies.html.
- Alia S. M.; Stariha S.; Borup R. L. Electrolyzer Durability at Low Catalyst Loading and with Dynamic Operation. J. Electrochem. Soc. 2019, 166 (15), F1164–F1172. 10.1149/2.0231915jes. [DOI] [Google Scholar]
- Pivovar B.; Ruth M.; Ahluwalia R.. H2NEW: Hydrogen (H2) from Next-Generation Electrolyzers of Water LTE Task 3c: System and Technoeconomic Analysis; National Renewable Energy Laboratories (NREL), 2022. [Google Scholar]
- Xi W.; Boyd M.; Ruth M.; Kurup P.; Xi W.; Boyd M.; Ruth M.; Kurup P.. Electrolyzers in the System Advisor Model (SAM): A Techno-Economic Potential Study; National Renewable Energy Laboratories (NREL), 2023. [Google Scholar]
- James B.; Colella W.; Moton J.; Saur G.; Ramsden T.. PEM Electrolysis H2A Production Case Study Documentation; U.S. Department of Energy, Fuel Cell Technologies Office, 2013. [Google Scholar]
- IRENA . Green Hydrogen Cost Reduction: Scaling up Electrolysers to Meet the 1.5°C Climate Goal; 2020. [Google Scholar]
- Hydrohub Innovation Program . Gigawatt Green Hydrogen Plant; 2020. [Google Scholar]
- Vicker J.; Peterson D.; Randolph K.. Cost of Electrolytic Hydrogen Production with Existing Technology; 2020. https://www.hydrogen.energy.gov/pdfs/20004-cost-electrolytic-hydrogen-production.pdf.
- Böhm H.; Zauner A.; Rosenfeld D. C.; Tichler R. Projecting Cost Development for Future Large-Scale Power-to-Gas Implementations by Scaling Effects. Appl. Energy 2020, 264, 114780. 10.1016/j.apenergy.2020.114780. [DOI] [Google Scholar]
- Saba S. M.; Muller M.; Robinius M.; Stolten D. The Investment Costs of Electrolysis: A Comparison of Cost Studies from the Past 30 Years. Int. J. Hydrogen Energy 2018, 43, 1209–1223. 10.1016/j.ijhydene.2017.11.115. [DOI] [Google Scholar]
- Bertuccilio L.; Chan A.; Hart D.; Lehner F.; Madden B.; Standen E.. Development of Water Electrolysis in the European Union; Fuel Cells and Hydrogen Joint Undertaking, 2014. [Google Scholar]
- Schmidt O.; Gambhir A.; Staffell I.; Hawkes A.; Nelson J.; Few S. Future Cost and Performance of Water Electrolysis: An Expert Elicitation Study. Int. J. Hydrogen Energy 2017, 42 (52), 30470–30492. 10.1016/j.ijhydene.2017.10.045. [DOI] [Google Scholar]
- Schmidt O.; Hawkes A.; Gambhir A.; Staffell I. The Future Cost of Electrical Energy Storage Based on Experience Rates. Nat. Energy 2017, 2, 17110. 10.1038/nenergy.2017.110. [DOI] [Google Scholar]
- Mayyas A.; Ruth M.; Pivovar B.; Bender G.; Wipke K.; Mayyas A.; Ruth M.; Pivovar B.; Bender G.; Wipke K.. Manufacturing Cost Analysis for Proton Exchange Membrane Water Electrolyzers; National Renewable Energy Laboratory, 2019.
- Badgett A.; Ruth M.; James B.; Pivovar B. Methods Identifying Cost Reduction Potential for Water Electrolysis Systems. Curr. Opin. Chem. Eng. 2021, 33, 100714. 10.1016/j.coche.2021.100714. [DOI] [Google Scholar]
- Tichler R.; Böhm H.; Zauner A.; Goers S.; Kroon P.. Innovative Large-Scale Energy Storage Tech-Nologies and Power-to-Gas Concepts after Optimization: Report on Experience Curves and Economies of Scale; 2018. [Google Scholar]
- Albrecht U.; Bünger U.; Michalski J.; Raksha T.; Wurster R.; Zerhusen J.. International Hydrogen Strategies; 2020. [Google Scholar]
- Fuel Cells and Hydrogen 2 Joint Undertaking Multi-Annual Work Plan 2014–2020; 2014; pp 1–78.
- Pivovar B. S.; Ruth M. F.; Myers D. J.; Dinh H. N. Hydrogen: Targeting $1/kg in 1 Decade. Electrochemical Society Interface 2021, 30 (4), 61–65. 10.1149/2.F15214IF. [DOI] [Google Scholar]
- Mayyas A.; Mann M. Emerging Manufacturing Technologies for Fuel Cells and Electrolyzers. Procedia Manuf 2019, 33, 508–515. 10.1016/j.promfg.2019.04.063. [DOI] [Google Scholar]
- Guo X.; Zhu H.; Zhang S. Overview of Electrolyser and Hydrogen Production Power Supply from Industrial Perspective. Int. J. Hydrogen Energy 2024, 49, 1048–1059. 10.1016/j.ijhydene.2023.10.325. [DOI] [Google Scholar]
- Wei M.; Lipman T.; Collella W.; James B. D.. A Total Cost of Ownership Model for Low Temperature PEM Fuel Cells in Combined Heat and Power and Backup Power Applications; 2014. [Google Scholar]
- Ayers K. E.Single Step Manufacturing of Low Catalyst Loading Electrolyzer MEAs; 2015. [Google Scholar]
- Pivovar B.H2NEW: Hydrogen (H2) from Next-Generation Electrolyzers of Water Overview; 2021. [Google Scholar]
- Lewinski K. A.; van der Vliet D.; Luopa S. M. NSTF Advances for PEM Electrolysis - the Effect of Alloying on Activity of NSTF Electrolyzer Catalysts and Performance of NSTF Based PEM Electrolyzers. ECS Meeting Abstracts 2015, MA2015-02 (37), 1457. 10.1149/MA2015-02/37/1457. [DOI] [Google Scholar]
- Ayers K.; Danilovic N.; Harrison K.; Xu H. PEM Electrolysis, a Forerunner for Clean Hydrogen. Electrochemical Society Interface 2021, 30 (4), 67–71. 10.1149/2.F16214IF. [DOI] [Google Scholar]
- Badgett A.; Ruth M.; Pivovar B.. Economic Considerations for Hydrogen Production with a Focus on Polymer Electrolyte Membrane Electrolysis; Elsevier B.V., 2021. [Google Scholar]
- Wang C.; Lee K.; Liu C. P.; Kulkarni D.; Atanassov P.; Peng X.; Zenyuk I. V. Design of PEM Water Electrolysers with Low Iridium Loading. International Materials Reviews 2024, 69 (1), 3–18. 10.1177/09506608231216665. [DOI] [Google Scholar]
- Wu Q.; Wang Y.; Zhang K.; Xie Z.; Sun K.; An W.; Liang X.; Zou X. Advances and Status of Anode Catalysts for Proton Exchange Membrane Water Electrolysis Technology. Mater. Chem. Front. 2023, 7, 1025–1045. 10.1039/D3QM00010A. [DOI] [Google Scholar]
- Song S.; Zhang H.; Ma X.; Shao Z.; Baker R. T.; Yi B. Electrochemical Investigation of Electrocatalysts for the Oxygen Evolution Reaction in PEM Water Electrolyzers. Int. J. Hydrogen Energy 2008, 33 (19), 4955–4961. 10.1016/j.ijhydene.2008.06.039. [DOI] [Google Scholar]
- Siracusano S.; Baglio V.; Grigoriev S. A.; Merlo L.; Fateev V. N.; Aricò A. S. The Influence of Iridium Chemical Oxidation State on the Performance and Durability of Oxygen Evolution Catalysts in PEM Electrolysis. J. Power Sources 2017, 366, 105–114. 10.1016/j.jpowsour.2017.09.020. [DOI] [Google Scholar]
- Mom R. V.; Falling L. J.; Kasian O.; Algara-Siller G.; Teschner D.; Crabtree R. H.; Knop-Gericke A.; Mayrhofer K. J. J.; Velasco-Vélez J. J.; Jones T. E. Operando Structure-Activity-Stability Relationship of Iridium Oxides during the Oxygen Evolution Reaction. ACS Catal. 2022, 12 (9), 5174–5184. 10.1021/acscatal.1c05951. [DOI] [Google Scholar]
- Rheinländer P. J.; Durst J. Transformation of the OER-Active IrOx Species under Transient Operation Conditions in PEM Water Electrolysis. J. Electrochem. Soc. 2021, 168 (2), 024511. 10.1149/1945-7111/abe0d4. [DOI] [Google Scholar]
- PLATINUM-GROUP METAL. https://d9-wret.s3.us-west-2.amazonaws.com/assets/palladium/production/mineral-pubs/platinum/mcs-2018-plati.pdf.
- Minke C.; Suermann M.; Bensmann B.; Hanke-Rauschenbach R. Is Iridium Demand a Potential Bottleneck in the Realization of Large-Scale PEM Water Electrolysis?. Int. J. Hydrogen Energy 2021, 46 (46), 23581–23590. 10.1016/j.ijhydene.2021.04.174. [DOI] [Google Scholar]
- Regmi Y. N.; Tzanetopoulos E.; Zeng G.; Peng X.; Kushner D. I.; Kistler T. A.; King L. A.; Danilovic N. Supported Oxygen Evolution Catalysts by Design: Toward Lower Precious Metal Loading and Improved Conductivity in Proton Exchange Membrane Water Electrolyzers. ACS Catal. 2020, 10 (21), 13125–13135. 10.1021/acscatal.0c03098. [DOI] [Google Scholar]
- Yu H.; Bonville L.; Jankovic J.; Maric R. Microscopic Insights on the Degradation of a PEM Water Electrolyzer with Ultra-Low Catalyst Loading. Appl. Catal., B 2020, 260, 118194. 10.1016/j.apcatb.2019.118194. [DOI] [Google Scholar]
- Siracusano S.; Hodnik N.; Jovanovic P.; Ruiz-Zepeda F.; Šala M.; Baglio V.; Aricò A. S. New Insights into the Stability of a High Performance Nanostructured Catalyst for Sustainable Water Electrolysis. Nano Energy 2017, 40, 618–632. 10.1016/j.nanoen.2017.09.014. [DOI] [Google Scholar]
- Taie Z.; Peng X.; Kulkarni D.; Zenyuk I. V.; Weber A. Z.; Hagen C.; Danilovic N. Pathway to Complete Energy Sector Decarbonization with Available Iridium Resources Using Ultralow Loaded Water Electrolyzers. ACS Appl. Mater. Interfaces 2020, 12, 52701. 10.1021/acsami.0c15687. [DOI] [PubMed] [Google Scholar]
- Yu H.; Danilovic N.; Wang Y.; Willis W.; Poozhikunnath A.; Bonville L.; Capuano C.; Ayers K.; Maric R. Nano-Size IrOx Catalyst of High Activity and Stability in PEM Water Electrolyzer with Ultra-Low Iridium Loading. Appl. Catal., B 2018, 239, 133–146. 10.1016/j.apcatb.2018.07.064. [DOI] [Google Scholar]
- Peng X.; Satjaritanun P.; Taie Z.; Wiles L.; Keane A.; Capuano C.; Zenyuk I. V.; Danilovic N. Insights into Interfacial and Bulk Transport Phenomena Affecting Proton Exchange Membrane Water Electrolyzer Performance at Ultra-Low Iridium Loadings. Adv. Sci. 2021, 8 (21), 2102950. 10.1002/advs.202102950. [DOI] [PMC free article] [PubMed] [Google Scholar]
- Schuler T.; De Bruycker R.; Schmidt T. J.; Büchi F. N. Polymer Electrolyte Water Electrolysis: Correlating Porous Transport Layer Structural Properties and Performance: Part I. Tomographic Analysis of Morphology and Topology. J. Electrochem. Soc. 2019, 166 (4), F270–F281. 10.1149/2.0561904jes. [DOI] [Google Scholar]
- Lee J. K.; Kim P.; Krause K.; Shrestha P.; Balakrishnan M.; Fahy K.; Fatih K.; Shaigan N.; Ge M.; Lee W. K.; Bazylak A. Designing Catalyst Layer Morphology for High-Performance Water Electrolysis Using Synchrotron X-Ray Nanotomography. Cell Rep. Phys. Sci. 2023, 4 (1), 101232. 10.1016/j.xcrp.2022.101232. [DOI] [Google Scholar]
- Schuler T.; Ciccone J.; Krentscher B.; Marone F.; Peter C.; Schmidt T.; Büchi F. Hierarchically Structured Porous Transport Layers for Polymer Electrolyte Water Electrolysis. Adv. Energy Mater. 2020, 10, 1903216. 10.1002/aenm.201903216. [DOI] [Google Scholar]
- Hegge F.; Lombeck F.; Ortiz E. C.; Bohn L.; von Holst M.; Kroschel M.; Hübner J.; Breitwieser M.; Strasser P.; Vierrath S. Efficient and Stable Low Iridium Loaded Anodes for PEM Water Electrolysis Made Possible by Nanofiber Interlayers. ACS Appl. Energy Mater. 2020, 3 (9), 8276–8284. 10.1021/acsaem.0c00735. [DOI] [Google Scholar]
- Chatterjee S.; Peng X.; Intikhab S.; Zeng G.; Kariuki N. N.; Myers D. J.; Danilovic N.; Snyder J. Nanoporous Iridium Nanosheets for Polymer Electrolyte Membrane Electrolysis. Adv. Energy Mater. 2021, 11 (34), 2101438. 10.1002/aenm.202101438. [DOI] [Google Scholar]
- Pourbaix M.Atlas of Electrochemical Equilibria In-Aqueous Solutions; National Association of Corrosion Engineers: Houston, TX, 1974. [Google Scholar]
- Polonský J.; Mazúr P.; Paidar M.; Christensen E.; Bouzek K. Performance of a PEM Water Electrolyser Using a TaC-Supported Iridium Oxide Electrocatalyst. Int. J. Hydrogen Energy 2014, 39 (7), 3072–3078. 10.1016/j.ijhydene.2013.12.085. [DOI] [Google Scholar]
- Karimi F.; Peppley B. A. Metal Carbide and Oxide Supports for Iridium-Based Oxygen Evolution Reaction Electrocatalysts for Polymer-Electrolyte-Membrane Water Electrolysis. Electrochim. Acta 2017, 246, 654–670. 10.1016/j.electacta.2017.06.048. [DOI] [Google Scholar]
- Hartig-Weiss A.; Miller M.; Beyer H.; Schmitt A.; Siebel A.; Freiberg A. T. S.; Gasteiger H. A.; El-Sayed H. A. Iridium Oxide Catalyst Supported on Antimony-Doped Tin Oxide for High Oxygen Evolution Reaction Activity in Acidic Media. ACS Appl. Nano Mater. 2020, 3 (3), 2185–2196. 10.1021/acsanm.9b02230. [DOI] [Google Scholar]
- Han B.; Risch M.; Belden S.; Lee S.; Bayer D.; Mutoro E.; Shao-Horn Y. Screening Oxide Support Materials for OER Catalysts in Acid. J. Electrochem. Soc. 2018, 165 (10), F813–F820. 10.1149/2.0921810jes. [DOI] [Google Scholar]
- Oh H. S.; Nong H. N.; Reier T.; Bergmann A.; Gliech M.; Araújo J. F. De; Willinger E.; Schlögl R.; Teschner D.; Strasser P. Electrochemical Catalyst-Support Effects and Their Stabilizing Role for IrOx Nanoparticle Catalysts during the Oxygen Evolution Reaction. J. Am. Chem. Soc. 2016, 138 (38), 12552–12563. 10.1021/jacs.6b07199. [DOI] [PubMed] [Google Scholar]
- Lin Y.; Dong Y.; Wang X.; Chen L. Electrocatalysts for Oxygen Evolution Reaction in Acidic Media. Adv. Mater. 2023, 35, 2210565. 10.1002/adma.202210565. [DOI] [PubMed] [Google Scholar]
- Reier T.; Nong H. N.; Teschner D.; Schlögl R.; Strasser P. Electrocatalytic Oxygen Evolution Reaction in Acidic Environments - Reaction Mechanisms and Catalysts. Adv. Energy Mater. 2017, 7 (1), 1601275. 10.1002/aenm.201601275. [DOI] [Google Scholar]
- Trasatti S. Electrocatalysis: Understanding the Success of DSA. Electrochim. Acta 2000, 45, 2377–2385. 10.1016/S0013-4686(00)00338-8. [DOI] [Google Scholar]
- Oakton E.; Lebedev D.; Povia M.; Abbott D. F.; Fabbri E.; Fedorov A.; Nachtegaal M.; Copéret C.; Schmidt T. J. IrO2-TiO2: A High-Surface-Area, Active, and Stable Electrocatalyst for the Oxygen Evolution Reaction. ACS Catal. 2017, 7 (4), 2346–2352. 10.1021/acscatal.6b03246. [DOI] [Google Scholar]
- Bernt M.; Siebel A.; Gasteiger H. A. Analysis of Voltage Losses in PEM Water Electrolyzers with Low Platinum Group Metal Loadings. J. Electrochem. Soc. 2018, 165 (5), F305–F314. 10.1149/2.0641805jes. [DOI] [Google Scholar]
- Bernt M.; Schramm C.; Schröter J.; Gebauer C.; Byrknes J.; Eickes C.; Gasteiger H. A. Effect of the IrOx Conductivity on the Anode Electrode/Porous Transport Layer Interfacial Resistance in PEM Water Electrolyzers. J. Electrochem. Soc. 2021, 168 (8), 084513. 10.1149/1945-7111/ac1eb4. [DOI] [Google Scholar]
- Möckl M.; Ernst M. F.; Kornherr M.; Allebrod F.; Bernt M.; Byrknes J.; Eickes C.; Gebauer C.; Moskovtseva A.; Gasteiger H. A. Durability Testing of Low-Iridium PEM Water Electrolysis Membrane Electrode Assemblies. J. Electrochem. Soc. 2022, 169 (6), 064505. 10.1149/1945-7111/ac6d14. [DOI] [Google Scholar]
- Möckl M.; Bernt M.; Schröter J.; Jossen A. Proton Exchange Membrane Water Electrolysis at High Current Densities: Investigation of Thermal Limitations. Int. J. Hydrogen Energy 2020, 45, 1417. 10.1016/j.ijhydene.2019.11.144. [DOI] [Google Scholar]
- Böhm D.; Beetz M.; Gebauer C.; Bernt M.; Schröter J.; Kornherr M.; Zoller F.; Bein T.; Fattakhova-Rohlfing D. Highly Conductive Titania Supported Iridium Oxide Nanoparticles with Low Overall Iridium Density as OER Catalyst for Large-Scale PEM Electrolysis. Appl. Mater. Today 2021, 24, 101134. 10.1016/j.apmt.2021.101134. [DOI] [Google Scholar]
- Othman M. A.; Amat N. F.; Ahmad B. H.; Rajan J. Electrical Conductivity Characteristic of TiO2 Nanowires From Hydrothermal Method. J. Phys. Conf Ser. 2014, 495 (1), 012027. 10.1088/1742-6596/495/1/012027. [DOI] [Google Scholar]
- Rozain C.; Mayousse E.; Guillet N.; Millet P. Influence of Iridium Oxide Loadings on the Performance of PEM Water Electrolysis Cells: Part II - Advanced Oxygen Electrodes. Appl. Catal., B 2016, 182, 123–131. 10.1016/j.apcatb.2015.09.011. [DOI] [Google Scholar]
- Siracusano S.; Baglio V.; D’Urso C.; Antonucci V.; Aricò A. S. Preparation and Characterization of Titanium Suboxides as Conductive Supports of IrO2 Electrocatalysts for Application in SPE Electrolysers. Electrochim. Acta 2009, 54 (26), 6292–6299. 10.1016/j.electacta.2009.05.094. [DOI] [Google Scholar]
- Böhm L.; Näther J.; Underberg M.; Kazamer N.; Holtkotte L.; Rost U.; Marginean G.; Wirkert F.; Brodmann M.; Hülser T.; Köster F. Pulsed Electrodeposition of Iridium Catalyst Nanoparticles on Titanium Suboxide Supports for Application in PEM Electrolysis. Mater. Today: Proc. 2021, 45, 4254–4259. 10.1016/j.matpr.2020.12.507. [DOI] [Google Scholar]
- Zhang L. M.; Gong Y. S.; Wang C. B.; Shen Q. Microstructure and Resistivity of Iridium Oxide Thin Films by Pulsed Laser Deposition Technique. Key Eng. Mater. 2007, 336–338, 2215–2217. 10.4028/www.scientific.net/KEM.336-338.2215. [DOI] [Google Scholar]
- Ryden W. D.; Lawson A. W.; Sartain C. C. Temperature Dependence of the Resistivity of RuO2 and IrO2. Phys. Lett. A 1968, 26 (5), 209–210. 10.1016/0375-9601(68)90126-6. [DOI] [Google Scholar]
- Mazúr P.; Polonský J.; Paidar M.; Bouzek K. Non-Conductive TiO2 as the Anode Catalyst Support for PEM Water Electrolysis. Int. J. Hydrogen Energy 2012, 37 (17), 12081–12088. 10.1016/j.ijhydene.2012.05.129. [DOI] [Google Scholar]
- Bernsmeier D.; Bernicke M.; Schmack R.; Sachse R.; Paul B.; Bergmann A.; Strasser P.; Ortel E.; Kraehnert R. Oxygen Evolution Catalysts Based on Ir-Ti Mixed Oxides with Templated Mesopore Structure: Impact of Ir on Activity and Conductivity. ChemSusChem 2018, 11 (14), 2367–2374. 10.1002/cssc.201800932. [DOI] [PubMed] [Google Scholar]
- Tran H. P.; Nong H. N.; Zlatar M.; Yoon A.; Hejral U.; Ruscher M.; Timoshenko J.; Selve S.; Berger D.; Kroschel M.; Klingenhof M.; Paul B.; Mohle S.; Nagi Nasralla K. N.; Escalera-Lopez D.; Bergmann A.; Cherevko S.; Cuenya B. R.; Strasser P. Reactivity and Stability of Reduced Ir-Weight TiO2-Supported Oxygen Evolution Catalysts for Proton Exchange Membrane (PEM) Water Electrolyzer Anodes. J. Am. Chem. Soc. 2024, 146 (46), 31444–31455. 10.1021/jacs.4c07002. [DOI] [PMC free article] [PubMed] [Google Scholar]
- De Angelis S.; Schuler T.; Sabharwal M.; Holler M.; Guizar-Sicairos M.; Müller E.; Büchi F. N. Understanding the Microstructure of a Core-Shell Anode Catalyst Layer for Polymer Electrolyte Water Electrolysis. Sci. Rep 2023, 13, 4280. 10.1038/s41598-023-30960-x. [DOI] [PMC free article] [PubMed] [Google Scholar]
- Pham C. V.; Bühler M.; Knöppel J.; Bierling M.; Seeberger D.; Escalera-López D.; Mayrhofer K. J. J.; Cherevko S.; Thiele S. IrO2 Coated TiO2 Core-Shell Microparticles Advance Performance of Low Loading Proton Exchange Membrane Water Electrolyzers. Appl. Catal., B 2020, 269, 118762. 10.1016/j.apcatb.2020.118762. [DOI] [Google Scholar]
- Alia S. M.; Reeves K. S.; Yu H.; Park J.; Kariuki N.; Kropf A. J.; Myers D. J.; Cullen D. A. Electrolyzer Performance Loss from Accelerated Stress Tests and Corresponding Changes to Catalyst Layers and Interfaces. J. Electrochem. Soc. 2022, 169 (5), 054517. 10.1149/1945-7111/ac697e. [DOI] [Google Scholar]
- Weiß A.; Siebel A.; Bernt M.; Shen T. H.; Tileli V.; Gasteiger H. A. Impact of Intermittent Operation on Lifetime and Performance of a PEM Water Electrolyzer. J. Electrochem. Soc. 2019, 166 (8), F487. 10.1149/2.0421908jes. [DOI] [Google Scholar]
- Grigoriev S. A.; Dzhus K. A.; Bessarabov D. G.; Millet P. Failure of PEM Water Electrolysis Cells: Case Study Involving Anode Dissolution and Membrane Thinning. Int. J. Hydrogen Energy 2014, 39 (35), 20440–20446. 10.1016/j.ijhydene.2014.05.043. [DOI] [Google Scholar]
- Milosevic M.; Böhm T.; Körner A.; Bierling M.; Winkelmann L.; Ehelebe K.; Hutzler A.; Suermann M.; Thiele S.; Cherevko S. In Search of Lost Iridium: Quantification of Anode Catalyst Layer Dissolution in Proton Exchange Membrane Water Electrolyzers. ACS Energy Lett. 2023, 8 (6), 2682–2688. 10.1021/acsenergylett.3c00193. [DOI] [Google Scholar]
- Raistrick I. D.Electrode Assembly for Use in a Solid Polymer Electrolyte Fuel Cell. US4876115A, 1989.
- Baker D. R.; Caulk D. A.; Neyerlin K. C.; Murphy M. W. Measurement of Oxygen Transport Resistance in PEM Fuel Cells by Limiting Current Methods. J. Electrochem. Soc. 2009, 156 (9), B991–B1003. 10.1149/1.3152226. [DOI] [Google Scholar]
- Greszler T. A.; Caulk D.; Sinha P. The Impact of Platinum Loading on Oxygen Transport Resistance. J. Electrochem. Soc. 2012, 159 (12), F831–F840. 10.1149/2.061212jes. [DOI] [Google Scholar]
- Weber A. Z.; Kusoglu A. Unexplained Transport Resistances for Low-Loaded Fuel-Cell Catalyst Layers. J. Mater. Chem. A Mater. 2014, 2 (41), 17207–17211. 10.1039/C4TA02952F. [DOI] [Google Scholar]
- Kongkanand A.; Mathias M. F. The Priority and Challenge of High-Power Performance of Low-Platinum Proton-Exchange Membrane Fuel Cells. J. Phys. Chem. Lett. 2016, 7 (7), 1127–1137. 10.1021/acs.jpclett.6b00216. [DOI] [PubMed] [Google Scholar]
- Gerhardt M. R.; Østenstad J. S.; Barnett A. O.; Thomassen M. S. Modeling Contact Resistance and Water Transport within a Cathode Liquid-Fed Proton Exchange Membrane Electrolyzer. J. Electrochem. Soc. 2023, 170 (12), 124516. 10.1149/1945-7111/ad129d. [DOI] [Google Scholar]
- Fornaciari J. C.; Gerhardt M. R.; Zhou J.; Regmi Y. N.; Danilovic N.; Bell A. T.; Weber A. Z. The Role of Water in Vapor-Fed Proton-Exchange-Membrane Electrolysis. J. Electrochem. Soc. 2020, 167 (10), 104508. 10.1149/1945-7111/ab9b09. [DOI] [Google Scholar]
- Lee J. K.; Anderson G.; Tricker A. W.; Babbe F.; Madan A.; Cullen D. A.; Arregui-Mena J. D.; Danilovic N.; Mukundan R.; Weber A. Z.; Peng X. Ionomer-Free and Recyclable Porous-Transport Electrode for High-Performing Proton-Exchange-Membrane Water Electrolysis. Nat. Commun. 2023, 14 (1), 4592. 10.1038/s41467-023-40375-x. [DOI] [PMC free article] [PubMed] [Google Scholar]
- Lee J. K.; Schuler T.; Bender G.; Sabharwal M.; Peng X.; Weber A. Z.; Danilovic N. Interfacial Engineering via Laser Ablation for High-Performing PEM Water Electrolysis. Appl. Energy 2023, 336, 120853. 10.1016/j.apenergy.2023.120853. [DOI] [Google Scholar]
- Alia S. M.; Reeves K. S.; Baxter J. S.; Cullen D. A. The Impact of Ink and Spray Variables on Catalyst Layer Properties, Electrolyzer Performance, and Electrolyzer Durability. J. Electrochem. Soc. 2020, 167 (14), 144512. 10.1149/1945-7111/abc746. [DOI] [Google Scholar]
- Creel E. B.; Tjiptowidjojo K.; Lee J. A.; Livingston K. M.; Schunk P. R.; Bell N. S.; Serov A.; Wood D. L. Slot-Die-Coating Operability Windows for Polymer Electrolyte Membrane Fuel Cell Cathode Catalyst Layers. J. Colloid Interface Sci. 2022, 610, 474–485. 10.1016/j.jcis.2021.11.047. [DOI] [PubMed] [Google Scholar]
- Serov A.; Kovnir K.; Shatruk M.; Kolen’ko Y. V. Critical Review of Platinum Group Metal-Free Materials for Water Electrolysis: Transition from the Laboratory to the Market: Earth-Abundant Borides and Phosphides as Catalysts for Sustainable Hydrogen Production. Johnson Matthey Technology Review 2021, 65 (2), 207–226. 10.1595/205651321X16067419458185. [DOI] [Google Scholar]
- Liu L. Platinum Group Metal Free Nano-Catalysts for Proton Exchange Membrane Water Electrolysis. Curr. Opin. Chem. Eng. 2021, 34, 100743. 10.1016/j.coche.2021.100743. [DOI] [Google Scholar]
- Bernt M.; Gasteiger H. A. Influence of Ionomer Content in IrO 2/TiO2 Electrodes on PEM Water Electrolyzer Performance. J. Electrochem. Soc. 2016, 163 (11), F3179–F3189. 10.1149/2.0231611jes. [DOI] [Google Scholar]
- Correa G.; Marocco P.; Muñoz P.; Falagüerra T.; Ferrero D.; Santarelli M. Pressurized PEM Water Electrolysis: Dynamic Modelling Focusing on the Cathode Side. Int. J. Hydrogen Energy 2022, 47 (7), 4315–4327. 10.1016/j.ijhydene.2021.11.097. [DOI] [Google Scholar]
- Bühre L. V.; McLeod A. J.; Trinke P.; Bensmann B.; Benecke M.; Herrera O. E.; Mérida W.; Hanke-Rauschenbach R. Adaptation of a PEMFC Reference Electrode to PEMWE: Possibilities and Limitations. J. Electrochem. Soc. 2023, 170 (9), 094507. 10.1149/1945-7111/acfac2. [DOI] [Google Scholar]
- Brightman E.; Dodwell J.; Van Dijk N.; Hinds G. In Situ Characterisation of PEM Water Electrolysers Using a Novel Reference Electrode. Electrochem commun 2015, 52, 1–4. 10.1016/j.elecom.2015.01.005. [DOI] [Google Scholar]
- Dodwell J.; Maier M.; Majasan J.; Jervis R.; Castanheira L.; Shearing P.; Hinds G.; Brett D. J. L. Open-Circuit Dissolution of Platinum from the Cathode in Polymer Electrolyte Membrane Water Electrolysers. J. Power Sources 2021, 498, 229937. 10.1016/j.jpowsour.2021.229937. [DOI] [Google Scholar]
- Rakousky C.; Reimer U.; Wippermann K.; Kuhri S.; Carmo M.; Lueke W.; Stolten D. Polymer Electrolyte Membrane Water Electrolysis: Restraining Degradation in the Presence of Fluctuating Power. J. Power Sources 2017, 342, 38–47. 10.1016/j.jpowsour.2016.11.118. [DOI] [Google Scholar]
- McLeod A. J.; Bühre L. V.; Bensmann B.; Herrera O. E.; Mérida W. Anode and Cathode Overpotentials under Accelerated Stress Testing of a PEM Electrolysis Cell. J. Power Sources 2024, 589, 233750. 10.1016/j.jpowsour.2023.233750. [DOI] [Google Scholar]
- Grigoriev S. A.; Bessarabov D. G.; Fateev V. N. Degradation Mechanisms of MEA Characteristics during Water Electrolysis in Solid Polymer Electrolyte Cells. Russian Journal of Electrochemistry 2017, 53 (3), 318–323. 10.1134/S1023193517030065. [DOI] [Google Scholar]
- Rakousky C.; Reimer U.; Wippermann K.; Carmo M.; Lueke W.; Stolten D. An Analysis of Degradation Phenomena in Polymer Electrolyte Membrane Water Electrolysis. J. Power Sources 2016, 326, 120–128. 10.1016/j.jpowsour.2016.06.082. [DOI] [Google Scholar]
- Chatenet M.; Pollet B. G.; Dekel D. R.; Dionigi F.; Deseure J.; Millet P.; Braatz R. D.; Bazant M. Z.; Eikerling M.; Staffell I.; Balcombe P.; Shao-Horn Y.; Schäfer H. Water Electrolysis: From Textbook Knowledge to the Latest Scientific Strategies and Industrial Developments. Chem. Soc. Rev. 2022, 51 (11), 4583–4762. 10.1039/D0CS01079K. [DOI] [PMC free article] [PubMed] [Google Scholar]
- Department of Energy Hydrogen and Fuel Cell Technologies Office . Bipartisan Infrastructure Law: Clean Hydrogen Electrolysis, Manufacturing, and Recycling; 2023. [Google Scholar]
- Trinke P.; Haug P.; Brauns J.; Bensmann B.; Hanke-Rauschenbach R.; Turek T. Hydrogen Crossover in PEM and Alkaline Water Electrolysis: Mechanisms, Direct Comparison and Mitigation Strategies. J. Electrochem. Soc. 2018, 165 (7), F502. 10.1149/2.0541807jes. [DOI] [Google Scholar]
- Hydrogen and Fuel Cell Technologies Office . Technical Targets for Proton Exchange Membrane Electrolysis. [Google Scholar]
- Kusoglu A.; Weber A. Z. New Insights into Perfluorinated Sulfonic-Acid Ionomers. Chem. Rev. 2017, 117 (3), 987–1104. 10.1021/acs.chemrev.6b00159. [DOI] [PubMed] [Google Scholar]
- Maalouf M.; Sun C.-N.; Pyle B.; Emery M.; Haugen G. M.; Hamrock S. J.; Zawodzinski T. A. Factors Enabling High Mobility of Protons and Water in Perfluorosulfonate Membranes under Low Hydration Conditions1. Int. J. Hydrogen Energy 2014, 39 (6), 2795–2800. 10.1016/j.ijhydene.2013.11.006. [DOI] [Google Scholar]
- Lewinski K. A.; van der Vliet D.; Luopa S. M. NSTF Advances for PEM Electrolysis - the Effect of Alloying on Activity of NSTF Electrolyzer Catalysts and Performance of NSTF Based PEM Electrolyzers. ECS Trans 2015, 69 (17), 893. 10.1149/06917.0893ecst. [DOI] [Google Scholar]
- Garbe S.; Futter J.; Schmidt T. J.; Gubler L. Insight into Elevated Temperature and Thin Membrane Application for High Efficiency in Polymer Electrolyte Water Electrolysis. Electrochim. Acta 2021, 377, 138046. 10.1016/j.electacta.2021.138046. [DOI] [Google Scholar]
- Mittelsteadt C. K.; Argun A.; Lacier C.; Willey J.. Dimensionally Stable High Performance Membranes. Annual Progress Report; 2016. https://www.hydrogen.energy.gov/docs/hydrogenprogramlibraries/pdfs/progress16/v_c_8_mittelsteadt_2016a714edd3-a30f-4568-a649-8357b784a6eb.pdf?sfvrsn=da73dd63_1
- Park A. M.; Gebhardt R.; Vander Woude M.; Wright B.; Plymill A.; Arslan F.; Gurau M.. Advanced Membranes for Improved Water Electrolyzer Performance. Towards the Next Generation of High Performance, Durable Water Electrolyzer Membranes. ECS Meeting Abstracts 2024, MA2024-01 ( (34), ), 1736. 10.1149/MA2024-01341736mtgabs [DOI] [Google Scholar]
- Siracusano S.; Pantò F.; Tonella S.; Oldani C.; Aricò A. S. Reinforced Short-Side-Chain Aquivion® Membrane for Proton Exchange Membrane Water Electrolysis. Int. J. Hydrogen Energy 2022, 47 (35), 15557–15570. 10.1016/j.ijhydene.2022.03.061. [DOI] [Google Scholar]
- Giancola S.; Zatoń M.; Reyes-Carmona Á.; Dupont M.; Donnadio A.; Cavaliere S.; Rozière J.; Jones D. J. Composite Short Side Chain PFSA Membranes for PEM Water Electrolysis. J. Membr. Sci. 2019, 570–571, 69–76. 10.1016/j.memsci.2018.09.063. [DOI] [Google Scholar]
- Albert A.; Barnett A. O.; Thomassen M. S.; Schmidt T. J.; Gubler L. Radiation-Grafted Polymer Electrolyte Membranes for Water Electrolysis Cells: Evaluation of Key Membrane Properties. ACS Appl. Mater. Interfaces 2015, 7 (40), 22203–22212. 10.1021/acsami.5b04618. [DOI] [PubMed] [Google Scholar]
- Stähler A.; Stähler M.; Scheepers F.; Lehnert W.; Carmo M. Scalable Implementation of Recombination Catalyst Layers to Mitigate Gas Crossover in PEM Water Electrolyzers. J. Electrochem. Soc. 2022, 169 (3), 034522. 10.1149/1945-7111/ac5c9b. [DOI] [Google Scholar]
- Omrani R.; Shabani B. Hydrogen Crossover in Proton Exchange Membrane Electrolysers: The Effect of Current Density, Pressure, Temperature, and Compression. Electrochim. Acta 2021, 377, 138085. 10.1016/j.electacta.2021.138085. [DOI] [Google Scholar]
- Kalinnikov A. A.; Grigoriev S. A.; Bessarabov D. G. Nonequilibrium Poroelectroelastic Theory for Polymer Electrolytes under Conditions of Water Electrolysis. Int. J. Hydrogen Energy 2019, 44 (16), 7889–7904. 10.1016/j.ijhydene.2019.02.025. [DOI] [Google Scholar]
- Schalenbach M.; Hoefner T.; Paciok P.; Carmo M.; Lueke W.; Stolten D. Gas Permeation through Nafion. Part 1: Measurements. J. Phys. Chem. C 2015, 119 (45), 25145–25155. 10.1021/acs.jpcc.5b04155. [DOI] [Google Scholar]
- Schalenbach M.; Hoeh M. A.; Gostick J. T.; Lueke W.; Stolten D. Gas Permeation through Nafion. Part 2: Resistor Network Model. J. Phys. Chem. C 2015, 119 (45), 25156–25169. 10.1021/acs.jpcc.5b04157. [DOI] [Google Scholar]
- Fumagalli M.; Lyonnard S.; Prajapati G.; Berrod Q.; Porcar L.; Guillermo A.; Gebel G. Fast Water Diffusion and Long-Term Polymer Reorganization during Nafion Membrane Hydration Evidenced by Time-Resolved Small-Angle Neutron Scattering. J. Phys. Chem. B 2015, 119 (23), 7068–7076. 10.1021/acs.jpcb.5b01220. [DOI] [PubMed] [Google Scholar]
- Bukola S.; Beard K.; Korzeniewski C.; Harris J. M.; Creager S. E. Single-Layer Graphene Sandwiched between Proton-Exchange Membranes for Selective Proton Transmission. ACS Appl. Nano Mater. 2019, 2 (2), 964–974. 10.1021/acsanm.8b02270. [DOI] [Google Scholar]
- Berning T.; Bessarabov D. GOMEA: A Conceptual Design of a Membrane Electrode Assembly for a Proton Exchange Membrane Electrolyzer. Membranes (Basel) 2023, 13 (7), 614. 10.3390/membranes13070614. [DOI] [PMC free article] [PubMed] [Google Scholar]
- Avdeenkov A. V.; Bessarabov D. G.; Zaryugin D. G. Passive Electrochemical Hydrogen Recombiner for Hydrogen Safety Systems: Prospects. Nuclear Science and Techniques 2023, 34 (6), 89. 10.1007/s41365-023-01245-9. [DOI] [Google Scholar]
- Schalenbach M.; Stolten D. High-Pressure Water Electrolysis: Electrochemical Mitigation of Product Gas Crossover. Electrochim. Acta 2015, 156, 321–327. 10.1016/j.electacta.2015.01.010. [DOI] [Google Scholar]
- Pantò F.; Siracusano S.; Briguglio N.; Aricò A. S. Durability of a Recombination Catalyst-Based Membrane-Electrode Assembly for Electrolysis Operation at High Current Density. Appl. Energy 2020, 279, 115809. 10.1016/j.apenergy.2020.115809. [DOI] [Google Scholar]
- Klose C.; Trinke P.; Böhm T.; Bensmann B.; Vierrath S.; Hanke-Rauschenbach R.; Thiele S. Membrane Interlayer with Pt Recombination Particles for Reduction of the Anodic Hydrogen Content in PEM Water Electrolysis. J. Electrochem. Soc. 2018, 165 (16), F1271–F1277. 10.1149/2.1241814jes. [DOI] [Google Scholar]
- Garbe S.; Babic U.; Nilsson E.; Schmidt T. J.; Gubler L. Communication—Pt-Doped Thin Membranes for Gas Crossover Suppression in Polymer Electrolyte Water Electrolysis. J. Electrochem. Soc. 2019, 166 (13), F873. 10.1149/2.0111913jes. [DOI] [Google Scholar]
- Uchida H.; Ueno Y.; Hagihara H.; Watanabe M. Self-Humidifying Electrolyte Membranes for Fuel Cells: Preparation of Highly Dispersed Particles in Nafion 112. J. Electrochem. Soc. 2003, 150 (1), A57. 10.1149/1.1523412. [DOI] [Google Scholar]
- Wang L.; Xing D. M.; Liu Y. H.; Cai Y. H.; Shao Z.-G.; Zhai Y. F.; Zhong H. X.; Yi B. L.; Zhang H. M. Pt/SiO2 Catalyst as an Addition to Nafion/PTFE Self-Humidifying Composite Membrane. J. Power Sources 2006, 161 (1), 61–67. 10.1016/j.jpowsour.2006.03.068. [DOI] [Google Scholar]
- Mukundan R.; Baker A. M.; Kusoglu A.; Beattie P.; Knights S.; Weber A. Z.; Borup R. L. Membrane Accelerated Stress Test Development for Polymer Electrolyte Fuel Cell Durability Validated Using Field and Drive Cycle Testing. J. Electrochem. Soc. 2018, 165 (6), F3085. 10.1149/2.0101806jes. [DOI] [Google Scholar]
- Bessarabov D. (Invited) Membranes with Recombination Catalyst for Hydrogen Crossover Reduction: Water Electrolysis. ECS Trans 2018, 85 (11), 17. 10.1149/08511.0017ecst. [DOI] [Google Scholar]
- Garbe S.; Samulesson E.; Schmidt T. J.; Gubler L. Comparison of Pt-Doped Membranes for Gas Crossover Suppression in Polymer Electrolyte Water Electrolysis. J. Electrochem. Soc. 2021, 168 (10), 104502. 10.1149/1945-7111/ac2925. [DOI] [Google Scholar]
- Scherer G. G.; Momose T.; Tomiie K. Membrel-Water Electrolysis Cells with a Fluorinated Cation Exchange Membrane. J. Electrochem. Soc. 1988, 135 (12), 3071. 10.1149/1.2095491. [DOI] [Google Scholar]
- Laconti A.; Liu H.; Mittelsteadt C.; McDonald R. Polymer Electrolyte Membrane Degradation Mechanisms in Fuel Cells - Findings Over the Past 30 Years and Comparison with Electrolyzers. ECS Trans 2006, 1 (8), 199. 10.1149/1.2214554. [DOI] [Google Scholar]
- Khatib F. N.; Wilberforce T.; Ijaodola O.; Ogungbemi E.; El-Hassan Z.; Durrant A.; Thompson J.; Olabi A. G. Material Degradation of Components in Polymer Electrolyte Membrane (PEM) Electrolytic Cell and Mitigation Mechanisms: A Review. Renewable and Sustainable Energy Reviews 2019, 111, 1–14. 10.1016/j.rser.2019.05.007. [DOI] [Google Scholar]
- Babic U.; Tarik M.; Schmidt T. J.; Gubler L. Understanding the Effects of Material Properties and Operating Conditions on Component Aging in Polymer Electrolyte Water Electrolyzers. J. Power Sources 2020, 451, 227778. 10.1016/j.jpowsour.2020.227778. [DOI] [Google Scholar]
- Tomić A. Z.; Pivac I.; Barbir F. A Review of Testing Procedures for Proton Exchange Membrane Electrolyzer Degradation. J. Power Sources 2023, 557, 232569. 10.1016/j.jpowsour.2022.232569. [DOI] [Google Scholar]
- Becker H.; Murawski J.; Shinde D. V.; Stephens I. E. L.; Hinds G.; Smith G. Impact of Impurities on Water Electrolysis: A Review. Sustain Energy Fuels 2023, 7 (7), 1565–1603. 10.1039/D2SE01517J. [DOI] [Google Scholar]
- Millet P.; Ranjbari A.; de Guglielmo F.; Grigoriev S. A.; Auprêtre F. Cell Failure Mechanisms in PEM Water Electrolyzers. Int. J. Hydrogen Energy 2012, 37 (22), 17478–17487. 10.1016/j.ijhydene.2012.06.017. [DOI] [Google Scholar]
- Fouda-Onana F.; Chandesris M.; Médeau V.; Chelghoum S.; Thoby D.; Guillet N. Investigation on the Degradation of MEAs for PEM Water Electrolysers Part I: Effects of Testing Conditions on MEA Performances and Membrane Properties. Int. J. Hydrogen Energy 2016, 41 (38), 16627–16636. 10.1016/j.ijhydene.2016.07.125. [DOI] [Google Scholar]
- Garbe S.; Futter J.; Agarwal A.; Tarik M.; Mularczyk A. A.; Schmidt T. J.; Gubler L. Understanding Degradation Effects of Elevated Temperature Operating Conditions in Polymer Electrolyte Water Electrolyzers. J. Electrochem. Soc. 2021, 168 (4), 44515. 10.1149/1945-7111/abf4ae. [DOI] [Google Scholar]
- Ayers K. E.; Anderson E. B.; Capuano C.; Carter B.; Dalton L.; Hanlon G.; Manco J.; Niedzwiecki M. Research Advances towards Low Cost, High Efficiency PEM Electrolysis. ECS Trans 2010, 33 (1), 3–15. 10.1149/1.3484496. [DOI] [Google Scholar]
- Arthurs C.; Kusoglu A. Compressive Creep of Polymer Electrolyte Membranes: A Case Study for Electrolyzers. ACS Appl. Energy Mater. 2021, 4 (4), 3249–3254. 10.1021/acsaem.0c03024. [DOI] [Google Scholar]
- Li N.; Araya S. S.; Cui X.; Kær S. K. The Effects of Cationic Impurities on the Performance of Proton Exchange Membrane Water Electrolyzer. J. Power Sources 2020, 473, 228617. 10.1016/j.jpowsour.2020.228617. [DOI] [Google Scholar]
- Wang X.; Zhang L.; Li G.; Zhang G.; Shao Z.-G.; Yi B. The Influence of Ferric Ion Contamination on the Solid Polymer Electrolyte Water Electrolysis Performance. Electrochim. Acta 2015, 158, 253–257. 10.1016/j.electacta.2015.01.140. [DOI] [Google Scholar]
- Sun S.; Shao Z.; Yu H.; Li G.; Yi B. Investigations on Degradation of the Long-Term Proton Exchange Membrane Water Electrolysis Stack. J. Power Sources 2014, 267, 515–520. 10.1016/j.jpowsour.2014.05.117. [DOI] [Google Scholar]
- Li N.; Araya S. S.; Kær S. K. Long-Term Contamination Effect of Iron Ions on Cell Performance Degradation of Proton Exchange Membrane Water Electrolyser. J. Power Sources 2019, 434, 226755. 10.1016/j.jpowsour.2019.226755. [DOI] [Google Scholar]
- Liu H.; Coms F. D.; Zhang J.; Gasteiger H. A.; LaConti A. B.. Chemical Degradation: Correlations Between Electrolyzer and Fuel Cell Findings. In Polymer Electrolyte Fuel Cell Durability; Büchi F. N.; Inaba M.; Schmidt T. J., Eds.; Springer New York: New York, NY, 2009; pp 71–118. [Google Scholar]
- Yandrasits M.New Fuel Cell Membranes with Improved Durability and Performance. In DOE Annual Merit Review; Washington, DC, 2017. [Google Scholar]
- Curtin D. E.; Lousenberg R. D.; Henry T. J.; Tangeman P. C.; Tisack M. E. Advanced Materials for Improved PEMFC Performance and Life. J. Power Sources 2004, 131 (1), 41–48. 10.1016/j.jpowsour.2004.01.023. [DOI] [Google Scholar]
- Xie T.; Hayden C. A. A Kinetic Model for the Chemical Degradation of Perfluorinated Sulfonic Acid Ionomers: Weak End Groups versus Side Chain Cleavage. Polymer (Guildf) 2007, 48 (19), 5497–5506. 10.1016/j.polymer.2007.07.043. [DOI] [Google Scholar]
- Ghassemzadeh L.; Peckham T. J.; Weissbach T.; Luo X.; Holdcroft S. Selective Formation of Hydrogen and Hydroxyl Radicals by Electron Beam Irradiation and Their Reactivity with Perfluorosulfonated Acid Ionomer. J. Am. Chem. Soc. 2013, 135 (42), 15923–15932. 10.1021/ja408032p. [DOI] [PubMed] [Google Scholar]
- Endoh E. Development of Highly Durable PFSA Membrane and MEA for PEMFC Under High Temperature and Low Humidity Conditions. ECS Trans 2008, 16 (2), 1229. 10.1149/1.2981964. [DOI] [Google Scholar]
- Danilczuk M.; Lancucki L.; Schlick S.; Hamrock S. J.; Haugen G. M. In-Depth Profiling of Degradation Processes in a Fuel Cell: 2D Spectral-Spatial FTIR Spectra of Nafion Membranes. ACS Macro Lett. 2012, 1 (2), 280–285. 10.1021/mz200100s. [DOI] [PubMed] [Google Scholar]
- Coms F. D. The Chemistry of Fuel Cell Membrane Chemical Degradation. ECS Trans 2008, 16 (2), 235–255. 10.1149/1.2981859. [DOI] [Google Scholar]
- Marocco P.; Sundseth K.; Aarhaug T.; Lanzini A.; Santarelli M.; Barnett A. O.; Thomassen M. Online Measurements of Fluoride Ions in Proton Exchange Membrane Water Electrolysis through Ion Chromatography. J. Power Sources 2021, 483, 229179. 10.1016/j.jpowsour.2020.229179. [DOI] [Google Scholar]
- Frensch S. H.; Fouda-Onana F.; Serre G.; Thoby D.; Araya S. S.; Kær S. K. Influence of the Operation Mode on PEM Water Electrolysis Degradation. Int. J. Hydrogen Energy 2019, 44 (57), 29889–29898. 10.1016/j.ijhydene.2019.09.169. [DOI] [Google Scholar]
- Zhang Z.; Han Z.; Testino A.; Gubler L. Platinum and Cerium-Zirconium Oxide Co-Doped Membrane for Mitigated H2 Crossover and Ionomer Degradation in PEWE. J. Electrochem. Soc. 2022, 169 (10), 104501. 10.1149/1945-7111/ac94a3. [DOI] [Google Scholar]
- Sun Q.; Yang F.; Jia Q.; Mittelsteadt C. The Impact of Cation Contamination on Proton Exchange Membrane Water Electrolyzer (PEMWE). ECS Meeting Abstracts 2023, MA2023-01 (36), 1962. 10.1149/MA2023-01361962mtgabs. [DOI] [Google Scholar]
- Sambandam S.; Ramani V. Influence of Binder Properties on Kinetic and Transport Processes in Polymer Electrolyte Fuel Cell Electrodes. Phys. Chem. Chem. Phys. 2010, 12 (23), 6140–6149. 10.1039/b921916a. [DOI] [PubMed] [Google Scholar]
- Kreuer K. D. On the Development of Proton Conducting Polymer Membranes for Hydrogen and Methanol Fuel Cells. J. Membr. Sci. 2001, 185 (1), 29–39. 10.1016/S0376-7388(00)00632-3. [DOI] [Google Scholar]
- Gottesfeld S.; Dekel D. R.; Page M.; Bae C.; Yan Y.; Zelenay P.; Kim Y. S. Anion Exchange Membrane Fuel Cells: Current Status and Remaining Challenges. J. Power Sources 2018, 375, 170–184. 10.1016/j.jpowsour.2017.08.010. [DOI] [Google Scholar]
- Klose C.; Saatkamp T.; Münchinger A.; Bohn L.; Titvinidze G.; Breitwieser M.; Kreuer K.-D.; Vierrath S. All-Hydrocarbon MEA for PEM Water Electrolysis Combining Low Hydrogen Crossover and High Efficiency. Adv. Energy Mater. 2020, 10 (14), 1903995. 10.1002/aenm.201903995. [DOI] [Google Scholar]
- Banan R.; Zu J.; Bazylak A. Humidity and Temperature Cycling Effects on Cracks and Delaminations in PEMFCs. Fuel Cells 2015, 15 (2), 327–336. 10.1002/fuce.201400118. [DOI] [Google Scholar]
- Kusoglu A.; Karlsson A. M.; Santare M. H.; Cleghorn S.; Johnson W. B. Mechanical Response of Fuel Cell Membranes Subjected to a Hygro-Thermal Cycle. J. Power Sources 2006, 161 (2), 987–996. 10.1016/j.jpowsour.2006.05.020. [DOI] [Google Scholar]
- Alavijeh A. S.; Bhattacharya S.; Thomas O.; Chuy C.; Yang Y.; Zhang H.; Kjeang E. Effect of Hygral Swelling and Shrinkage on Mechanical Durability of Fuel Cell Membranes. J. Power Sources 2019, 427, 207–214. 10.1016/j.jpowsour.2019.04.081. [DOI] [Google Scholar]
- Han S.-Y.; Yu D. M.; Mo Y.-H.; Ahn S. M.; Lee J. Y.; Kim T.-H.; Yoon S. J.; Hong S.; Hong Y. T.; So S. Ion Exchange Capacity Controlled Biphenol-Based Sulfonated Poly(Arylene Ether Sulfone) for Polymer Electrolyte Membrane Water Electrolyzers: Comparison of Random and Multi-Block Copolymers. J. Membr. Sci. 2021, 634, 119370. 10.1016/j.memsci.2021.119370. [DOI] [Google Scholar]
- Kusoglu A.; Weber A. Z. A Mechanistic Model for Pinhole Growth in Fuel-Cell Membranes during Cyclic Loads. J. Electrochem. Soc. 2014, 161 (8), E3311 10.1149/2.036408jes. [DOI] [Google Scholar]
- Kusoglu A.; Santare M. H.; Karlsson A. M. Aspects of Fatigue Failure Mechanisms in Polymer Fuel Cell Membranes. J. Polym. Sci. B Polym. Phys. 2011, 49 (21), 1506–1517. 10.1002/polb.22336. [DOI] [Google Scholar]
- Kreitmeier S.; Lerch P.; Wokaun A.; Büchi F. N. Local Degradation at Membrane Defects in Polymer Electrolyte Fuel Cells. J. Electrochem. Soc. 2013, 160 (4), F456. 10.1149/1.023306jes. [DOI] [Google Scholar]
- Weber A. Z. Gas-Crossover and Membrane-Pinhole Effects in Polymer-Electrolyte Fuel Cells. J. Electrochem. Soc. 2008, 155 (6), B521. 10.1149/1.2898130. [DOI] [Google Scholar]
- Bender G.; Felt W.; Ulsh M. Detecting and Localizing Failure Points in Proton Exchange Membrane Fuel Cells Using IR Thermography. J. Power Sources 2014, 253, 224–229. 10.1016/j.jpowsour.2013.12.045. [DOI] [Google Scholar]
- Kusoglu A.; Calabrese M.; Weber A. Z. Effect of Mechanical Compression on Chemical Degradation of Nafion Membranes. ECS Electrochemistry Letters 2014, 3 (5), F33. 10.1149/2.008405eel. [DOI] [Google Scholar]
- Hong S. J.; Jung H. Y.; Yoon S. J.; Oh K.-H.; Oh S.-G.; Hong Y. T.; Yu D. M.; So S. Constrained Hydrocarbon-Based Ionomers in Porous Poly(Tetrafluoroethylene) Supports for Enhanced Durability of Polymer Electrolyte Membrane Fuel Cells and Water Electrolyzers. J. Power Sources 2022, 551, 232221. 10.1016/j.jpowsour.2022.232221. [DOI] [Google Scholar]
- Noh Y. S.; Jeong H. Y.; Kim T.-H.; Choi J.; Lee J. Y.; So S.; Yu D. M. Sulfonated Poly(p-Phenylene)-Based Ionomer/PTFE Composite Membrane with Enhanced Performance and Durability for Energy Conversion Devices. J. Power Sources 2023, 580, 233422. 10.1016/j.jpowsour.2023.233422. [DOI] [Google Scholar]
- Scherer G. G. Polymer Membranes for Fuel Cells. Berichte der Bunsengesellschaft für physikalische Chemie 1990, 94 (9), 1008–1014. 10.1002/bbpc.19900940926. [DOI] [Google Scholar]
- Wang X.; Mardle P.; Adamski M.; Chen B.; Holdcroft S. Proton Exchange Membrane Water Electrolysis Incorporating Sulfo-Phenylated Polyphenylene Catalyst Coated Membranes. J. Electrochem. Soc. 2023, 170 (2), 024502. 10.1149/1945-7111/acb643. [DOI] [Google Scholar]
- Choi S.; Shin S.-H.; Lee D.-H.; Doo G.; Lee D. W.; Hyun J.; Lee J. Y.; Kim H.-T. Enhancing the Durability of Hydrocarbon-Membrane-Based Polymer Electrolyte Water Electrolysis Using a Radical Scavenger-Embedded Interlocking Interfacial Layer. J. Mater. Chem. A Mater. 2022, 10 (2), 789–798. 10.1039/D1TA08222A. [DOI] [Google Scholar]
- Gubler L.; Nauser T.; Coms F. D.; Lai Y.-H.; Gittleman C. S. Perspective—Prospects for Durable Hydrocarbon-Based Fuel Cell Membranes. J. Electrochem. Soc. 2018, 165 (6), F3100. 10.1149/2.0131806jes. [DOI] [Google Scholar]
- Kodama K.; Motobayashi K.; Shinohara A.; Hasegawa N.; Kudo K.; Jinnouchi R.; Osawa M.; Morimoto Y. Effect of the Side-Chain Structure of Perfluoro-Sulfonic Acid Ionomers on the Oxygen Reduction Reaction on the Surface of Pt. ACS Catal. 2018, 8 (1), 694–700. 10.1021/acscatal.7b03571. [DOI] [Google Scholar]
- Chowdhury A.; Bird A.; Liu J.; Zenyuk I. V.; Kusoglu A.; Radke C. J.; Weber A. Z. Linking Perfluorosulfonic Acid Ionomer Chemistry and High-Current Density Performance in Fuel-Cell Electrodes. ACS Appl. Mater. Interfaces 2021, 13 (36), 42579–42589. 10.1021/acsami.1c07611. [DOI] [PubMed] [Google Scholar]
- Li D.; Chung H. T.; Maurya S.; Matanovic I.; Kim Y. S. Impact of Ionomer Adsorption on Alkaline Hydrogen Oxidation Activity and Fuel Cell Performance. Curr. Opin Electrochem 2018, 12, 189–195. 10.1016/j.coelec.2018.11.012. [DOI] [Google Scholar]
- Maurya S.; Noh S.; Matanovic I.; Park E. J.; Narvaez Villarrubia C.; Martinez U.; Han J.; Bae C.; Kim Y. S. Rational Design of Polyaromatic Ionomers for Alkaline Membrane Fuel Cells with > 1 W cm–2 Power Density. Energy Environ. Sci. 2018, 11 (11), 3283–3291. 10.1039/C8EE02192A. [DOI] [Google Scholar]
- Trinke P.; Keeley G. P.; Carmo M.; Bensmann B.; Hanke-Rauschenbach R. Elucidating the Effect of Mass Transport Resistances on Hydrogen Crossover and Cell Performance in PEM Water Electrolyzers by Varying the Cathode Ionomer Content. J. Electrochem. Soc. 2019, 166 (8), F465. 10.1149/2.0171908jes. [DOI] [Google Scholar]
- Sambandam S.; Ramani V. In Situ Measurement of Oxygen Permeability in Polymer Electrolyte Membranes. ECS Trans 2009, 25 (1), 433. 10.1149/1.3210593. [DOI] [Google Scholar]
- Sambandam S.; Parrondo J.; Ramani V. Estimation of Electrode Ionomer Oxygen Permeability and Ionomer-Phase Oxygen Transport Resistance in Polymer Electrolyte Fuel Cells. Phys. Chem. Chem. Phys. 2013, 15 (36), 14994–15002. 10.1039/c3cp51450a. [DOI] [PubMed] [Google Scholar]
- Chuy C.; Basura V. I.; Simon E.; Holdcroft S.; Horsfall J.; Lovell K. V. Electrochemical Characterization of Ethylenetetrafluoroethylene-g-polystyrenesulfonic Acid Solid Polymer Electrolytes. J. Electrochem. Soc. 2000, 147 (12), 4453. 10.1149/1.1394085. [DOI] [Google Scholar]
- Park E.; Jannasch P.; Miyatake K.; Bae C.; Noonan K.; Fujimoto C.; Holdcroft S.; Varcoe J.; Henkensmeier D.; Guiver M.; Kim Y. Aryl Ether-Free Polymer Electrolytes for Electrochemical and Energy Devices. Chem. Soc. Rev. 2024, 53, 5704. 10.1039/D3CS00186E. [DOI] [PubMed] [Google Scholar]
- Kim Y. S.; Pivovar B. S. The Membrane-Electrode Interface in PEFCs: IV. The Origin and Implications of Interfacial Resistance. J. Electrochem. Soc. 2010, 157 (11), B1616. 10.1149/1.3481581. [DOI] [Google Scholar]
- Kang S.; Jeong H.; Yoon S. J.; So S.; Choi J.; Kim T.; Yu D. Hydrocarbon-Based Composite Membrane Using LCP-Nonwoven Fabrics for Durable Proton Exchange Membrane Water Electrolysis. Polymers (Basel) 2023, 15, 2109. 10.3390/polym15092109. [DOI] [PMC free article] [PubMed] [Google Scholar]
- Nguyen H.; Lombeck F.; Schwarz C.; Heizmann P. A.; Adamski M.; Lee H. F.; Britton B.; Holdcroft S.; Vierrath S.; Breitwieser M. Hydrocarbon-Based PemionTM Proton Exchange Membrane Fuel Cells with State-of-the-Art Performance. Sustain Energy Fuels 2021, 5 (14), 3687–3699. 10.1039/D1SE00556A. [DOI] [Google Scholar]
- Peron J.; Shi Z.; Holdcroft S. Hydrocarbon Proton Conducting Polymers for Fuel Cell Catalyst Layers. Energy Environ. Sci. 2011, 4 (5), 1575–1591. 10.1039/c0ee00638f. [DOI] [Google Scholar]
- Strong A.; Britton B.; Edwards D.; Peckham T. J.; Lee H.-F.; Huang W. Y.; Holdcroft S. Alcohol-Soluble, Sulfonated Poly(Arylene Ether)s: Investigation of Hydrocarbon Ionomers for Proton Exchange Membrane Fuel Cell Catalyst Layers. J. Electrochem. Soc. 2015, 162 (6), F513. 10.1149/2.0251506jes. [DOI] [Google Scholar]
- Balogun E.; Adamski M.; Holdcroft S. Communication—Non-Fluorous, Hydrocarbon PEMFCs, Generating > 1 W cm–2 Power. J. Electrochem. Soc. 2020, 167 (8), 84502. 10.1149/1945-7111/ab88bd. [DOI] [Google Scholar]
- Astill T.; Xie Z.; Shi Z.; Navessin T.; Holdcroft S. Factors Influencing Electrochemical Properties and Performance of Hydrocarbon-Based Electrolyte PEMFC Catalyst Layers. J. Electrochem. Soc. 2009, 156 (4), B499. 10.1149/1.3082119. [DOI] [Google Scholar]
- Chae J. E.; Yoo S. J.; Kim J. Y.; Jang J. H.; Lee S. Y.; Song K. H.; Kim H.-J. Hydrocarbon-Based Electrode Ionomer for Proton Exchange Membrane Fuel Cells. Int. J. Hydrogen Energy 2020, 45 (57), 32856–32864. 10.1016/j.ijhydene.2020.03.003. [DOI] [Google Scholar]
- Nguyen H.; Klose C.; Metzler L.; Vierrath S.; Breitwieser M. Fully Hydrocarbon Membrane Electrode Assemblies for Proton Exchange Membrane Fuel Cells and Electrolyzers: An Engineering Perspective. Adv. Energy Mater. 2022, 12 (12), 2103559. 10.1002/aenm.202103559. [DOI] [Google Scholar]
- Kulkarni D.; Huynh A.; Satjaritanun P.; O’Brien M.; Shimpalee S.; Parkinson D.; Shevchenko P.; DeCarlo F.; Danilovic N.; Ayers K. E.; Capuano C.; Zenyuk I. V. Elucidating Effects of Catalyst Loadings and Porous Transport Layer Morphologies on Operation of Proton Exchange Membrane Water Electrolyzers. Appl. Catal., B 2022, 308, 121213. 10.1016/j.apcatb.2022.121213. [DOI] [Google Scholar]
- Lopata J.; Kang Z.; Young J.; Bender G.; Weidner J. W.; Shimpalee S. Effects of the Transport/Catalyst Layer Interface and Catalyst Loading on Mass and Charge Transport Phenomena in Polymer Electrolyte Membrane Water Electrolysis Devices. J. Electrochem. Soc. 2020, 167 (6), 064507. 10.1149/1945-7111/ab7f87. [DOI] [Google Scholar]
- Yuan X. Z.; Shaigan N.; Song C.; Aujla M.; Neburchilov V.; Kwan J. T. H.; Wilkinson D. P.; Bazylak A.; Fatih K. The Porous Transport Layer in Proton Exchange Membrane Water Electrolysis: Perspectives on a Complex Component. Sustain Energy Fuels 2022, 6 (8), 1824–1853. 10.1039/D2SE00260D. [DOI] [Google Scholar]
- Stiber S.; Sata N.; Morawietz T.; Ansar S. A.; Jahnke T.; Lee J. K.; Bazylak A.; Fallisch A.; Gago A. S.; Friedrich K. A. A High-Performance, Durable and Low-Cost Proton Exchange Membrane Electrolyser with Stainless Steel Components. Energy Environ. Sci. 2022, 15 (1), 109–122. 10.1039/D1EE02112E. [DOI] [Google Scholar]
- Doan T. L.; Lee H. E.; Shah S. S. H.; Kim M. J.; Kim C. H.; Cho H. S.; Kim T. A Review of the Porous Transport Layer in Polymer Electrolyte Membrane Water Electrolysis. Int. J. Energy Res. 2021, 45 (10), 14207–14220. 10.1002/er.6739. [DOI] [Google Scholar]
- Hackemüller F. J.; Borgardt E.; Panchenko O.; Müller M.; Bram M. Manufacturing of Large-Scale Titanium-Based Porous Transport Layers for Polymer Electrolyte Membrane Electrolysis by Tape Casting. Adv. Eng. Mater. 2019, 21 (6), 1–10. 10.1002/adem.201801201. [DOI] [Google Scholar]
- Lettenmeier P.; Kolb S.; Sata N.; Fallisch A.; Zielke L.; Thiele S.; Gago A. S.; Friedrich K. A. Comprehensive Investigation of Novel Pore-Graded Gas Diffusion Layers for High-Performance and Cost-Effective Proton Exchange Membrane Electrolyzers. Energy Environ. Sci. 2017, 10 (12), 2521–2533. 10.1039/C7EE01240C. [DOI] [Google Scholar]
- Lang J. T.; Kulkarni D.; Foster C. W.; Huang Y.; Sepe M. A.; Shimpalee S.; Parkinson D. Y.; Zenyuk I. V. X-Ray Tomography Applied to Electrochemical Devices and Electrocatalysis. Chem. Rev. 2023, 123 (16), 9880–9914. 10.1021/acs.chemrev.2c00873. [DOI] [PMC free article] [PubMed] [Google Scholar]
- Majasan J. O.; Iacoviello F.; Shearing P. R.; Brett D. J. L. Effect of Microstructure of Porous Transport Layer on Performance in Polymer Electrolyte Membrane Water Electrolyser. Energy Procedia 2018, 151, 111–119. 10.1016/j.egypro.2018.09.035. [DOI] [Google Scholar]
- Kulkarni D.Interfaces in Polymer Electrolyte Membrane Water Electrolyzers. Ph.D. Dissertation, University of California, Irvine, 2022. [Google Scholar]
- Kulkarni D.; Ouimet R.; Erb B.; Parkinson D. Y.; Chang H.-M.; Wang C.; Smeltz A.; Capuano C.; Zenyuk I. V. Influence of Microporous Layers on Interfacial Properties, Oxygen Flow Distribution, and Durability of Proton Exchange Membrane Water Electrolyzers. ACS Appl. Mater. Interfaces 2023, 15 (41), 48060–48071. 10.1021/acsami.3c06899. [DOI] [PubMed] [Google Scholar]
- Liu C.; Shviro M.; Gago A. S.; Zaccarine S. F.; Bender G.; Gazdzicki P.; Morawietz T.; Biswas I.; Rasinski M.; Everwand A.; Schierholz R.; Pfeilsticker J.; Müller M.; Lopes P. P.; Eichel R. A.; Pivovar B.; Pylypenko S.; Friedrich K. A.; Lehnert W.; Carmo M. Exploring the Interface of Skin-Layered Titanium Fibers for Electrochemical Water Splitting. Adv. Energy Mater. 2021, 11 (8), 2002926. 10.1002/aenm.202002926. [DOI] [Google Scholar]
- Lee C. H.; Lee J. K.; Zhao B.; Fahy K. F.; LaManna J. M.; Baltic E.; Hussey D. S.; Jacobson D. L.; Schulz V. P.; Bazylak A. Temperature-Dependent Gas Accumulation in Polymer Electrolyte Membrane Electrolyzer Porous Transport Layers. J. Power Sources 2020, 446, 227312. 10.1016/j.jpowsour.2019.227312. [DOI] [Google Scholar]
- Steen S. M.; Mo J.; Kang Z.; Yang G.; Zhang F. Y. Investigation of Titanium Liquid/Gas Diffusion Layers in Proton Exchange Membrane Electrolyzer Cells. Int. J. Green Energy 2017, 14 (2), 162–170. 10.1080/15435075.2016.1253582. [DOI] [Google Scholar]
- Kroschel M.; Bonakdarpour A.; Kwan J. T. H.; Strasser P.; Wilkinson D. P. Analysis of Oxygen Evolving Catalyst Coated Membranes with Different Current Collectors Using a New Modified Rotating Disk Electrode Technique. Electrochim. Acta 2019, 317, 722–736. 10.1016/j.electacta.2019.05.011. [DOI] [Google Scholar]
- Choi H.; Kim O.-H.; Kim M.; Choe H.; Cho Y.-H.; Sung Y.-E. Next-Generation Polymer-Electrolyte-Membrane Fuel Cells Using Titanium Foam as Gas Diffusion Layer. ACS Appl. Mater. Interfaces 2014, 6 (10), 7665–7671. 10.1021/am500962h. [DOI] [PubMed] [Google Scholar]
- Stiber S.; Balzer H.; Wierhake A.; Wirkert F. J.; Roth J.; Rost U.; Brodmann M.; Lee J. K.; Bazylak A.; Waiblinger W.; Gago A. S.; Friedrich K. A. Porous Transport Layers for Proton Exchange Membrane Electrolysis Under Extreme Conditions of Current Density, Temperature, and Pressure. Adv. Energy Mater. 2021, 11 (33), 1–11. 10.1002/aenm.202100630. [DOI] [Google Scholar]
- Ma T.-C.; Hutzler A.; Bensmann B.; Hanke-Rauschenbach R.; Thiele S. Influence of the Complex Interface between Transport and Catalyst Layer on Water Electrolysis Performance. J. Electrochem. Soc. 2024, 171, 044504. 10.1149/1945-7111/ad3497. [DOI] [Google Scholar]
- Weber C. C.; Wrubel J. A.; Gubler L.; Bender G.; De Angelis S.; Büchi F. N. How the Porous Transport Layer Interface Affects Catalyst Utilization and Performance in Polymer Electrolyte Water Electrolysis. ACS Appl. Mater. Interfaces 2023, 15 (29), 34750–34763. 10.1021/acsami.3c04151. [DOI] [PMC free article] [PubMed] [Google Scholar]
- Sepe M.; Lopata J.; Madkour S.; Mayerhoefer B.; Ciesielski A.; Siljanovska-Petreska G.; Nestle N.; Shimpalee S. Multiscale Three-Dimensional Modeling of Two-Phase Transport inside Porous Transport Layers. Int. J. Hydrogen Energy 2024, 59, 1143–1155. 10.1016/j.ijhydene.2024.02.070. [DOI] [Google Scholar]
- Schuler T.; Schmidt T. J.; Büchi F. N. Polymer Electrolyte Water Electrolysis: Correlating Performance and Porous Transport Layer Structure: Part II. Electrochemical Performance Analysis. J. Electrochem. Soc. 2019, 166 (10), F555. 10.1149/2.1241908jes. [DOI] [Google Scholar]
- Ferner K. J.; Park J.; Kang Z.; Mauger S. A.; Ulsh M.; Bender G.; Litster S. Morphological Analysis of Iridium Oxide Anode Catalyst Layers for Proton Exchange Membrane Water Electrolysis Using High-Resolution Imaging. Int. J. Hydrogen Energy 2024, 59, 176–186. 10.1016/j.ijhydene.2024.02.020. [DOI] [Google Scholar]
- Lee J. K.; Lee C.; Fahy K. F.; Kim P. J.; Krause K.; LaManna J. M.; Baltic E.; Jacobson D. L.; Hussey D. S.; Bazylak A. Accelerating Bubble Detachment in Porous Transport Layers with Patterned through Pores. ACS Appl. Energy Mater. 2020, 3 (10), 9676–9684. 10.1021/acsaem.0c01239. [DOI] [Google Scholar]
- Suermann M.; Gimpel T.; Bühre L. V.; Schade W.; Bensmann B.; Hanke-Rauschenbach R. Femtosecond Laser-Induced Surface Structuring of the Porous Transport Layers in Proton Exchange Membrane Water Electrolysis. J. Mater. Chem. A Mater. 2020, 8 (9), 4898–4910. 10.1039/C9TA12127G. [DOI] [Google Scholar]
- Leonard E.; Shum A. D.; Normile S.; Sabarirajan D. C.; Yared D. G.; Xiao X.; Zenyuk I. V. Operando X-Ray Tomography and Sub-Second Radiography for Characterizing Transport in Polymer Electrolyte Membrane Electrolyzer. Electrochim. Acta 2018, 276, 424–433. 10.1016/j.electacta.2018.04.144. [DOI] [Google Scholar]
- Lee J. K.; Lee C. H.; Fahy K. F.; Zhao B.; LaManna J. M.; Baltic E.; Jacobson D. L.; Hussey D. S.; Bazylak A. Critical Current Density as a Performance Indicator for Gas-Evolving Electrochemical Devices. Cell Rep. Phys. Sci. 2020, 1 (8), 100147. 10.1016/j.xcrp.2020.100147. [DOI] [Google Scholar]
- Seweryn J.; Biesdorf J.; Schmidt T. J.; Boillat P. Communication—Neutron Radiography of the Water/Gas Distribution in the Porous Layers of an Operating Electrolyser. J. Electrochem. Soc. 2016, 163 (11), F3009–F3011. 10.1149/2.0641607jes. [DOI] [Google Scholar]
- Mo J.; Kang Z.; Retterer S. T.; Cullen D. A.; Toops T. J.; Green J. B.; Mench M. M.; Zhang F.-Y. Discovery of True Electrochemical Reactions for Ultrahigh Catalyst Mass Activity in Water Splitting. Sci. Adv. 2016, 2 (11), 1600690. 10.1126/sciadv.1600690. [DOI] [PMC free article] [PubMed] [Google Scholar]
- Lee J. K.; Lee C. H.; Bazylak A. Pore Network Modelling to Enhance Liquid Water Transport through Porous Transport Layers for Polymer Electrolyte Membrane Electrolyzers. J. Power Sources 2019, 437, 226910. 10.1016/j.jpowsour.2019.226910. [DOI] [Google Scholar]
- Lee J. K.; Bazylak A. Optimizing Porous Transport Layer Design Parameters via Stochastic Pore Network Modelling: Reactant Transport and Interfacial Contact Considerations. J. Electrochem. Soc. 2020, 167 (1), 013541. 10.1149/1945-7111/ab6557. [DOI] [Google Scholar]
- Jung S.; Sabharwal M.; Jarauta A.; Wei F.; Gingras M.; Gostick J.; Secanell M. Estimation of Relative Transport Properties in Porous Transport Layers Using Pore-Scale and Pore-Network Simulations. J. Electrochem. Soc. 2021, 168 (6), 064501. 10.1149/1945-7111/ac03f2. [DOI] [Google Scholar]
- Lee J. K.; Lee C.; Fahy K. F.; Kim P. J.; LaManna J. M.; Baltic E.; Jacobson D. L.; Hussey D. S.; Stiber S.; Gago A. S.; Friedrich K. A.; Bazylak A. Spatially Graded Porous Transport Layers for Gas Evolving Electrochemical Energy Conversion: High Performance Polymer Electrolyte Membrane Electrolyzers. Energy Convers Manag 2020, 226, 113545. 10.1016/j.enconman.2020.113545. [DOI] [PMC free article] [PubMed] [Google Scholar]
- Moore M.; Mandal M.; Kosakian A.; Secanell M. Numerical Study of the Impact of Two-Phase Flow in the Anode Catalyst Layer on the Performance of Proton Exchange Membrane Water Electrolysers. J. Electrochem. Soc. 2023, 170 (4), 044503. 10.1149/1945-7111/acc898. [DOI] [Google Scholar]
- Zhao B.; Lee C. H.; Lee J. K.; Fahy K. F.; LaManna J. M.; Baltic E.; Jacobson D. L.; Hussey D. S.; Bazylak A. Superhydrophilic Porous Transport Layer Enhances Efficiency of Polymer Electrolyte Membrane Electrolyzers. Cell Rep. Phys. Sci. 2021, 2 (10), 100580. 10.1016/j.xcrp.2021.100580. [DOI] [Google Scholar]
- Lettenmeier P.; Kolb S.; Burggraf F.; Gago A. S.; Friedrich K. A. Towards Developing a Backing Layer for Proton Exchange Membrane Electrolyzers. J. Power Sources 2016, 311, 153–158. 10.1016/j.jpowsour.2016.01.100. [DOI] [Google Scholar]
- Kang Z.; Yang G.; Mo J.; Yu S.; Cullen D. A.; Retterer S. T.; Toops T. J.; Brady M. P.; Bender G.; Pivovar B. S.; Green J. B.; Zhang F. Y. Developing Titanium Micro/Nano Porous Layers on Planar Thin/Tunable LGDLs for High-Efficiency Hydrogen Production. Int. J. Hydrogen Energy 2018, 43 (31), 14618. 10.1016/j.ijhydene.2018.05.139. [DOI] [Google Scholar]
- Rakousky C.; Keeley G. P.; Wippermann K.; Carmo M.; Stolten D. The Stability Challenge on the Pathway to High-Current-Density Polymer Electrolyte Membrane Water Electrolyzers. Electrochim. Acta 2018, 278, 324–331. 10.1016/j.electacta.2018.04.154. [DOI] [Google Scholar]
- Liu C.; Carmo M.; Bender G.; Everwand A.; Lickert T.; Young J. L.; Smolinka T.; Stolten D.; Lehnert W. Performance Enhancement of PEM Electrolyzers through Iridium-Coated Titanium Porous Transport Layers. Electrochem commun 2018, 97, 96–99. 10.1016/j.elecom.2018.10.021. [DOI] [Google Scholar]
- Liu C.; Wippermann K.; Rasinski M.; Suo Y.; Shviro M.; Carmo M.; Lehnert W. Constructing a Multifunctional Interface between Membrane and Porous Transport Layer for Water Electrolyzers. ACS Appl. Mater. Interfaces 2021, 13 (14), 16182–16196. 10.1021/acsami.0c20690. [DOI] [PubMed] [Google Scholar]
- Fan Z.; Yu H.; Jiang G.; Yao D.; Sun S.; Chi J.; Qin B.; Shao Z. Low Precious Metal Loading Porous Transport Layer Coating and Anode Catalyst Layer for Proton Exchange Membrane Water Electrolysis. Int. J. Hydrogen Energy 2022, 47 (44), 18963–18971. 10.1016/j.ijhydene.2022.04.114. [DOI] [Google Scholar]
- Bystron T.; Vesely M.; Paidar M.; Papakonstantinou G.; Sundmacher K.; Bensmann B.; Hanke-Rauschenbach R.; Bouzek K. Enhancing PEM Water Electrolysis Efficiency by Reducing the Extent of Ti Gas Diffusion Layer Passivation. J. Appl. Electrochem. 2018, 48 (6), 713–723. 10.1007/s10800-018-1174-6. [DOI] [Google Scholar]
- Bautkinova T.; Utsch N.; Bystron T.; Lhotka M.; Kohoutkova M.; Shviro M.; Bouzek K. Introducing Titanium Hydride on Porous Transport Layer for More Energy Efficient Water Electrolysis with Proton Exchange Membrane. J. Power Sources 2023, 565, 232913. 10.1016/j.jpowsour.2023.232913. [DOI] [Google Scholar]
- Zenyuk I.; Parkinson D.; Connolly L.; Weber A. Gas-Diffusion-Layer Structural Properties under Compression via X-Ray Tomography. J. Power Sources 2016, 328, 364–376. 10.1016/j.jpowsour.2016.08.020. [DOI] [Google Scholar]
- Zenyuk I. V.; Parkinson D. Y.; Hwang G.; Weber A. Z. Probing Water Distribution in Compressed Fuel-Cell Gas-Diffusion Layers Using X-Ray Computed Tomography. Electrochem commun 2015, 53, 24–28. 10.1016/j.elecom.2015.02.005. [DOI] [Google Scholar]
- Zenyuk I. V.; Lamibrac A.; Eller J.; Parkinson D. Y.; Marone F.; Büchi F. N.; Weber A. Z. Investigating Evaporation in Gas Diffusion Layers for Fuel Cells with X-Ray Computed Tomography. J. Phys. Chem. C 2016, 120 (50), 28701–28711. 10.1021/acs.jpcc.6b10658. [DOI] [Google Scholar]
- Atkinson R.; Garsany Y.; Gould B.; Swider-Lyons K.; Zenyuk I. The Role of Compressive Stress on Gas Diffusion Media Morphology and Fuel Cell Performance. ACS Appl. Energy Mater. 2018, 1, 191. 10.1021/acsaem.7b00077. [DOI] [Google Scholar]
- Gago A. S.; Ansar A. S.; Gazdzicki P.; Wagner N.; Arnold J.; Friedrich K. A. Low Cost Bipolar Plates for Large Scale PEM Electrolyzers. ECS Meeting Abstracts 2014, MA2014-02 (21), 1236–1236. 10.1149/MA2014-02/21/1236. [DOI] [Google Scholar]
- Gago A. S.; Ansar S. A.; Saruhan B.; Schulz U.; Lettenmeier P.; Cañas N. A.; Gazdzicki P.; Morawietz T.; Hiesgen R.; Arnold J.; Friedrich K. A. Protective Coatings on Stainless Steel Bipolar Plates for Proton Exchange Membrane (PEM) Electrolysers. J. Power Sources 2016, 307, 815–825. 10.1016/j.jpowsour.2015.12.071. [DOI] [Google Scholar]
- Teuku H.; Alshami I.; Goh J.; Masdar M. S.; Loh K. S. Review on Bipolar Plates for Low-Temperature Polymer Electrolyte Membrane Water Electrolyzer. Int. J. Energy Res. 2021, 45 (15), 20583–20600. 10.1002/er.7182. [DOI] [Google Scholar]
- Rojas N.; Sánchez-Molina M.; Sevilla G.; Amores E.; Almandoz E.; Esparza J.; Cruz Vivas M. R.; Colominas C. Coated Stainless Steels Evaluation for Bipolar Plates in PEM Water Electrolysis Conditions. Int. J. Hydrogen Energy 2021, 46 (51), 25929–25943. 10.1016/j.ijhydene.2021.03.100. [DOI] [Google Scholar]
- Gago A. S.; Ansar A. S.; Gazdzicki P.; Wagner N.; Arnold J.; Friedrich K. A. Low Cost Bipolar Plates for Large Scale PEM Electrolyzers. ECS Trans 2014, 64 (3), 1039. 10.1149/06403.1039ecst. [DOI] [Google Scholar]
- Leng Y.; Ming P.; Yang D.; Zhang C. Stainless Steel Bipolar Plates for Proton Exchange Membrane Fuel Cells: Materials, Flow Channel Design and Forming Processes. J. Power Sources 2020, 451, 227783. 10.1016/j.jpowsour.2020.227783. [DOI] [Google Scholar]
- Hu Q.; Zhang D.; Fu H.; Huang K. Investigation of Stamping Process of Metallic Bipolar Plates in PEM Fuel Cell - Numerical Simulation and Experiments. Int. J. Hydrogen Energy 2014, 39 (25), 13770–13776. 10.1016/j.ijhydene.2014.01.201. [DOI] [Google Scholar]
- Barzegari M. M.; Khatir F. A. Study of Thickness Distribution and Dimensional Accuracy of Stamped Metallic Bipolar Plates. Int. J. Hydrogen Energy 2019, 44 (59), 31360–31371. 10.1016/j.ijhydene.2019.09.225. [DOI] [Google Scholar]
- Khatir F. A.; Elyasi M.; Ghadikolaee H. T.; Hosseinzadeh M. Evaluation of Effective Parameters on Stamping of Metallic Bipolar Plates. Procedia Eng. 2017, 183, 322–329. 10.1016/j.proeng.2017.04.047. [DOI] [Google Scholar]
- Ayers K.High Performance, Low Cost Hydrogen Generation from Renewable Energy; 2012. [Google Scholar]
- Roy R.; Critz K.; Leonida A.. Electrode Plate Structures For High-Pressure Electrochemical Cell Devices. US 6171719 B1, 2001.
- Ni A.; Upadhyay M.; Kumar S. S.; Uwitonze H.; Lim H. Anode Analysis and Modelling Hydrodynamic Behaviour of the Multiphase Flow Field in Circular PEM Water Electrolyzer. Int. J. Hydrogen Energy 2023, 48 (43), 16176–16183. 10.1016/j.ijhydene.2023.01.032. [DOI] [Google Scholar]
- Nie J.; Chen Y.; Cohen S.; Carter B. D.; Boehm R. F. Numerical and Experimental Study of Three-Dimensional Fluid Flow in the Bipolar Plate of a PEM Electrolysis Cell. International Journal of Thermal Sciences 2009, 48 (10), 1914–1922. 10.1016/j.ijthermalsci.2009.02.017. [DOI] [Google Scholar]
- Lin R.; Lu Y.; Xu J.; Huo J.; Cai X. Investigation on Performance of Proton Exchange Membrane Electrolyzer with Different Flow Field Structures. Appl. Energy 2022, 326, 120011. 10.1016/j.apenergy.2022.120011. [DOI] [Google Scholar]
- Wang X. Y.; Wang Z. M.; Feng Y. C.; Xu C.; Chen Z. C.; Liao Z. R.; Ju X. Three-Dimensional Multiphase Modeling of a Proton Exchange Membrane Electrolysis Cell with a New Interdigitated-Jet Hole Flow Field. Sci. China Technol. Sci. 2022, 65 (5), 1179–1192. 10.1007/s11431-022-2026-6. [DOI] [Google Scholar]
- Olesen A. C.; Frensch S. H.; Kær S. K. Towards Uniformly Distributed Heat, Mass and Charge: A Flow Field Design Study for High Pressure and High Current Density Operation of PEM Electrolysis Cells. Electrochim. Acta 2019, 293, 476–495. 10.1016/j.electacta.2018.10.008. [DOI] [Google Scholar]
- Wei Q.; Fan L.; Tu Z. Hydrogen Production in a Proton Exchange Membrane Electrolysis Cell (PEMEC) with Titanium Meshes as Flow Distributors. Int. J. Hydrogen Energy 2023, 48 (93), 36271–36285. 10.1016/j.ijhydene.2023.06.052. [DOI] [Google Scholar]
- Wilhelm Sievers G.; Anklam K.; Henkel R.; Hickmann T.; Brüser V. Corrosion-Protection of Moulded Graphite Conductive Plastic Bipolar Plates in PEM Electrolysis by Plasma Processing. Int. J. Hydrogen Energy 2019, 44 (5), 2435–2445. 10.1016/j.ijhydene.2018.12.020. [DOI] [Google Scholar]
- LaConti A. B.; Swette L.. Handbook of Fuel Cells - Fundamentals, Technology and Applications, Vol. 55; Vielstich W.; Gasteiger H. A.; Lamm A., Eds.; John Wiley & Sons, 2003. [Google Scholar]
- Hamdan M.PEM Electrolyzer Incorporating an Advanced Low Cost Membrane; 2013, 10.2172/1091385. [DOI] [Google Scholar]
- Oudenhuijzen M. K.; Bitter J. H.; Koningsberger D. C. The Nature of the Pt-H Bonding for Strongly and Weakly Bonded Hydrogen on Platinum. A XAFS Spectroscopy Study of the Pt-H Antibonding Shaperesonance and Pt-H EXAFS. J. Phys. Chem. B 2001, 105 (20), 4616–4622. 10.1021/jp0108014. [DOI] [Google Scholar]
- Wang C.Corrosion Resistant and Electrically Conductive Surface of Metallic Components for Electrolyzers. WO 2014/169134 A2, 2014.
- Cavaliere P. Water Electrolysis for Hydrogen Production 2023, 10.1007/978-3-031-37780-8. [DOI] [Google Scholar]
- Kuhnert E.; Hacker V.; Bodner M. A Review of Accelerated Stress Tests for Enhancing MEA Durability in PEM Water Electrolysis Cells. Int. J. Energy Res. 2023, 2023, 1–23. 10.1155/2023/3183108. [DOI] [Google Scholar]
- Bazarah A.; Majlan E. H.; Husaini T.; Zainoodin A. M.; Alshami I.; Goh J.; Masdar M. S. Factors Influencing the Performance and Durability of Polymer Electrolyte Membrane Water Electrolyzer: A Review. Int. J. Hydrogen Energy 2022, 47 (85), 35976–35989. 10.1016/j.ijhydene.2022.08.180. [DOI] [Google Scholar]
- U.S. Department of Energy . Fuel Cell Technologies Office Multi-Year Research, Development, and Demonstration Plan - Section 3.4 Fuel Cells; U.S. Department of Energy, Washington, D.C., 2016, https://www.energy.gov/sites/prod/files/2017/05/f34/fcto_myrdd_fuel_cells.pdf. [Google Scholar]
- Stariha S.; Macauley N.; Sneed B. T.; Langlois D.; More K. L.; Mukundan R.; Borup R. L. Recent Advances in Catalyst Accelerated Stress Tests for Polymer Electrolyte Membrane Fuel Cells. J. Electrochem. Soc. 2018, 165 (7), F492–F501. 10.1149/2.0881807jes. [DOI] [Google Scholar]
- Commission E.; Centre J. R.; Tsotridis G.; Pilenga A.. EU Harmonized Protocols for Testing of Low Temperature Water Electrolysis; Publications Office, 2021. 10.2760/58880. [DOI] [Google Scholar]
- Aßmann P.; Gago A. S.; Gazdzicki P.; Friedrich K. A.; Wark M. Toward Developing Accelerated Stress Tests for Proton Exchange Membrane Electrolyzers. Curr. Opin Electrochem 2020, 21, 225–233. 10.1016/j.coelec.2020.02.024. [DOI] [Google Scholar]
- Myers D. J.; Wang X.; Smith M. C.; More K. L. Potentiostatic and Potential Cycling Dissolution of Polycrystalline Platinum and Platinum Nano-Particle Fuel Cell Catalysts. J. Electrochem. Soc. 2018, 165 (6), F3178–F3190. 10.1149/2.0211806jes. [DOI] [Google Scholar]
- Borup R.; Davey J.; Garzon F.; Wood D. III; Inbody M. PEM Fuel Cell Electrocatalyst Durability Measurements. J. Power Sources 2006, 163, 76–81. 10.1016/j.jpowsour.2006.03.009. [DOI] [Google Scholar]
- Voronova A.; Kim H. J.; Jang J. H.; Park H. Y.; Seo B. Effect of Low Voltage Limit on Degradation Mechanism during High-Frequency Dynamic Load in Proton Exchange Membrane Water Electrolysis. Int. J. Energy Res. 2022, 46 (9), 11867–11878. 10.1002/er.7953. [DOI] [Google Scholar]
- Stucki S.; Scherer G. G.; Schlagowski S.; Fischer E. PEM Water Electrolysers: Evidence for Membrane Failure in 100kW Demonstration Plants. J. Appl. Electrochem. 1998, 28 (10), 1041–1049. 10.1023/A:1003477305336. [DOI] [Google Scholar]
- Chandesris M.; Médeau V.; Guillet N.; Chelghoum S.; Thoby D.; Fouda-Onana F. Membrane Degradation in PEM Water Electrolyzer: Numerical Modeling and Experimental Evidence of the Influence of Temperature and Current Density. Int. J. Hydrogen Energy 2015, 40 (3), 1353–1366. 10.1016/j.ijhydene.2014.11.111. [DOI] [Google Scholar]
- Tang H.; Peikang S.; Jiang S.; Wang F.; Pan M. A Degradation Study of Nafion Proton Exchange Membrane of PEM Fuel Cells. J. Power Sources 2007, 170, 85–92. 10.1016/j.jpowsour.2007.03.061. [DOI] [Google Scholar]
- Chen J.; Goshtasbi A.; Soleymani A.; Ricketts M.; Waldecker J.; Xu C.; Yang J.; Ersal T.; Jankovic J. Effects of Cycle Duration and Test Hardware in Relative Humidity Cycling of a Polymer Electrolyte Membrane. J. Power Sources 2020, 476, 228576. 10.1016/j.jpowsour.2020.228576. [DOI] [Google Scholar]
- Kandlikar S. G.; Garofalo M. L.; Lu Z. Water Management in a PEMFC: Water Transport Mechanism and Material Degradation in Gas Diffusion Layers. Fuel Cells 2011, 11, 814–823. 10.1002/fuce.201000172. [DOI] [Google Scholar]
- Perry M.; Patterson T.; Madden T. GDL Degradation in PEFC. ECS Transactions 2010, 33, 1081. 10.1149/1.3484601. [DOI] [Google Scholar]
- Toyota . Toyota to Accelerate Plant Decarbonization Efforts in Fukushima Using Hydrogen; 2023.
- Tashie-Lewis B. C.; Nnabuife S. G. Hydrogen Production, Distribution, Storage and Power Conversion in a Hydrogen Economy - A Technology Review. Chemical Engineering Journal Advances 2021, 8, 100172. 10.1016/j.ceja.2021.100172. [DOI] [Google Scholar]
- Proost J. State-of-the Art CAPEX Data for Water Electrolysers, and Their Impact on Renewable Hydrogen Price Settings. Int. J. Hydrogen Energy 2019, 44 (9), 4406–4413. 10.1016/j.ijhydene.2018.07.164. [DOI] [Google Scholar]
- Ouimet R. J.; Glenn J. R.; De Porcellinis D.; Motz A. R.; Carmo M.; Ayers K. E. The Role of Electrocatalysts in the Development of Gigawatt-Scale PEM Electrolyzers. ACS Catal. 2022, 12 (10), 6159–6171. 10.1021/acscatal.2c00570. [DOI] [Google Scholar]
- U.S. Department of Energy .Water Electrolyzers and Fuel Cells Supply Chain; 2022.
- Mittelsteadt C.; Sorensen E.; Jia Q. Ir Strangelove, or How to Learn to Stop Worrying and Love the PEM Water Electrolysis. Energy Fuels 2023, 37 (17), 12558–12569. 10.1021/acs.energyfuels.3c01524. [DOI] [Google Scholar]
- Clapp M.; Zalitis C. M.; Ryan M. Green Hydrogen via PEM Electrolysis - Avoiding Iridium Supply Limitations. ECS Trans 2023, 111 (4), 21. 10.1149/11104.0021ecst. [DOI] [Google Scholar]
- Pritchard D. K.; Royle M.; Willoughby D.. Installation Permitting Guidance For Hydrogen and Fuel Cell Stationary Applications: UK Version; Health and Safety Laboratory: Buxton, United Kingdom, 2009.
- Vacin G. B.; Eckerle T.; Kashuba M.. Hydrogen Station Permitting Guidebook; California Governor’s Office of Business and Economic Development, 2020. [Google Scholar]
- HINICIO . Deliverable: Study on the Possibilities to Produce, Use and Export “Green” Hydrogen in Costa Rica, ver. 3; 2021. [Google Scholar]
- Nasser M.; Megahed T.; Ookawara S.; Hassan H. A Review of Water Electrolysis-Based Systems for Hydrogen Production Using Hybrid/Solar/Wind Energy Systems. Environ. Sci. Pollut. Res. 2022, 29, 86994. 10.1007/s11356-022-23323-y. [DOI] [PMC free article] [PubMed] [Google Scholar]
- Green Hydrogen in China: A Roadmap for Progress; World Economic Forum, 2023. [Google Scholar]
- Clean Hydrogen Joint Undertaking. Clean Hydrogen Joint Undertaking. Strategic Research and Innovation Agenda 2021–2027; 2022. [Google Scholar]
- Bernuy-Lopez C.Electrolysis technologies and LCOH: current state and prospects for 2030; Hydrogen Tech World, 2023. [Google Scholar]
- Peng X.; Taie Z.; Liu J.; Zhang Y.; Peng X.; Regmi Y. N.; Fornaciari J. C.; Capuano C.; Binny D.; Kariuki N. N.; Myers D. J.; Scott M. C.; Weber A. Z.; Danilovic N. Hierarchical Electrode Design of Highly Efficient and Stable Unitized Regenerative Fuel Cells (URFCs) for Long-Term Energy Storage. Energy Environ. Sci. 2020, 13 (12), 4872–4881. 10.1039/D0EE03244A. [DOI] [Google Scholar]