Skip to main content
Scientific Reports logoLink to Scientific Reports
. 2025 May 25;15:18234. doi: 10.1038/s41598-025-01685-w

Comparison of 3D printed and conventional denture base materials in terms of durability and performance characteristics

Zeynep Öztürk 1,✉, Büşra Tosun 2
PMCID: PMC12104351  PMID: 40414931

Abstract

The aim of this study was to compare the performance of denture base materials produced by three-dimensional (3D) printing and conventional methods in terms of their mechanical durability and water absorption and solubility properties. Conventional polymethyl methacrylate (PMMA) samples (Meliodent, Heraeus Kulzer, Germany) were prepared using the pressing technique. PowerResins (3BFAB Technology, Inc., Istanbul, Turkey) was used to produce the 3D printed denture base samples. The 3D printed samples were designed using Meshmixer software (Autodesk, Inc.) and printed on a DentaFab Sega 3D Printer (DentaFab, Istanbul, Turkey). Flexural and compressive strength and microhardness tests were conducted to evaluate the mechanical properties of the samples. Water absorption and solubility tests were also performed. The flexural and compressive strength and microhardness values ​​of the 3D printed group were higher than those of the conventional group (p < 0.001). The mean water absorption value was lower in the 3D printed group compared to the conventional group, and the difference between these values ​​was statistically significant (p < 0.001). A statistically significant difference was noted between the groups in terms of water solubility ​​(p = 0.003). Our study shows that 3D printing can produce customized and high-precision prosthetic bases while also improving their physical and mechanical properties.

Keywords: Additive manufacturing, 3D printers, Mechanical testing, Water absorption, Water solubility

Subject terms: Medical research, Materials science

Introduction

Digital technology holds an important place in modern dentistry1. The use of three-dimensional (3D) printers involves technological processes in which a 3D model, either created personally or available, is printed solidly. These printers provide a clean and safe production process and reduce production times. Additional advantages include digital storage and production with a low margin of error2,3. The use of 3D printing has contributed to the development and implementation of new treatment and diagnostic methods in different specialties of dentistry. Its adoption has increased significantly, especially in areas such as prosthetic dentistry, pediatric dentistry, and orthodontics. In these areas, 3D printing technology has begun to be preferred as an alternative to traditional applications1,4–6. This technology improves patient comfort and satisfaction by providing better fit and occlusion stability compared to conventional methods. It has the potential to improve treatment processes by offering high precision, aesthetic advantages, and faster production processes thanks to personalized production1,7. The integration of existing knowledge and experience with this emerging technology can enable dentists to more easily apply accurate and effective treatment methods while offering patients a wider range of treatments and increasing satisfaction rates. The widespread use of 3D printing in clinical applications has great potential to improve patient experience, optimize treatment times, and offer individualized solutions by creating a powerful alternative to conventional treatment methods8.

Polymethyl methacrylate (PMMA) is a denture base material that has been widely used since the 1940s. It is known for its biocompatibility, color stability, and minimal water absorption9,10.​ PMMA-based denture bases have gained an important place in dentistry because they provide aesthetic and functional solutions for patients with missing teeth. They are widely used in prosthetic dental treatments and the production of toothed and edentulous removable space maintainers and children’s dentures1. Although the use of heat-polymerized (conventional) PMMA is very common, its production involves a difficult and time-consuming laboratory process11–13. The mechanical properties of the prosthetic base materials directly affect the durability, lifespan, and patient comfort of the prosthesis in clinical practice14. Disadvantages, such as polymerization shrinkage and mechanical strength limitations, have emerged over time, and the development of different compositions and processing techniques is on the agenda to overcome these deficiencies13,15–18.

The use of 3D printing technology is increasing in denture base production. With digital design and 3D printing, denture bases that perfectly fit the anatomical structure of each patient are being produced. This technology thus allows customization to the individual needs of each patient19,20.

Contradictory results have been found in studies that compared the mechanical properties of denture base materials produced by conventional and 3D printing methods. In general, it has been reported that the physicochemical properties of denture base materials produced by 3D printing are lower than those produced by traditional methods16,21,22. However, studies have also indicated that this difference can be eliminated by extending the curing time of23,24 or taking different approaches to the material composition17,20.

The aim of the present study was to reveal the potential advantages of the 3D printing method in dentistry by comparing the mechanical properties and water absorption and solubility of conventional and 3D printed denture base materials. The null hypothesis of this study was that there is no difference between the performance properties of the denture base materials produced by the 3D printing method and those produced by the conventional method.

Materials and methods

Sample size calculation

We carried out a power analysis using the G*Power software program (version 3.0.10, Heinrich Heine University Düsseldorf), which showed that at least 26 samples were required for the highest power level (power = 80, a = 0.05). Four extra samples were prepared, which resulted in 30 samples for the 3D printed group and 30 samples for the conventional group (Table 1). A total of 240 specimens (60/ Flexure strength tests, 60/ microhardness test, 60/ compressive strength tests and 60/water absorption and solubility test) were distributed into two groups: control (conventional PMMA) and experimental group (3D printed PMMA).

Table 1.

Protocol of power analysis.

Parameter Value
Test type F tests—ANOVA: Fixed effects, omnibus, one-way
Analize type A priori: Compute required sample size
Effect size (f) 0.40
α err prob 0.05
Power (1 + β) 0.80
Number of groups 2
Noncentrality parameter λ 8.32
Critical F 4.0343097
Numerator df 1
Denominator df 50
Total sample size 52
Actual power 0.8074866

Sample design and Preparation

Compression molding technique procedures were followed to prepare conventional PMMA specimens. Wax specimens were prepared using 3D-printed specimens as reference molds to ensure better accuracy for each test group. Gypsum was poured into the lower half of the flask, and wax templates were placed inside. After induration, the first layer of gypsum was covered with a separating fluid (Separating Fluid, Ivoclar Vivadent, Liechtenstein). The remaining part of the flask was covered with gypsum and sealed. After the gypsum setting, the wax was removed by placing it in boiling water. Acrylic resin (Meliodent, Heraeus Kulzer, Germany) was prepared and adapted to the cavity created using the lost wax technique with the powder/liquid ratio determined following the manufacturer’s instructions and placed in the hydraulic press for 5 min. Then, the flasks were placed in hot water and the molds were completely covered with water and polymerized at 100 °C for 20 min. Afterward, the molds were cooled slowly in a water bath. After cooling, the polymerized samples were removed from the mold. The excess acrylic test samples were trimmed16. All the samples were finalized by processing with 600, 800, and 1200 grit grinding paper at 300 rpm under a water coolant for 30 s each. The thickness of each sample was checked with a digital caliper (Digimatic AOS, Mituyoto AG, Japan) with a precision of 0.001 mm23.

The 3D printed denture base material PowerResins (3BFAB Technology, Inc., Istanbul, Turkey) was used in this study. The 3D samples were designed using Meshmixer software (Autodesk, Inc.). The generated standard tessellation language (STL) files were adapted, and the created file was exported to the printer’s slicing software. The samples were printed using a DentaFab Sega 3D Printer (DentaFab, Istanbul, Turkey). During the sample production phase, all the printing parameters were standardized to 100 μm layer thickness25, a standard support type, and a 90° printing angle11,26. After printing, the samples were washed in a washing unit (Medifive Twin Cure, South Korea) containing 95% ethanol in accordance with the manufacturer’s instructions for 5 min and then dried with an air water spray. The samples were cured using a UV light polymerization unit with a curing light wavelength range of 365–405 nm for 30 min (Medifive Twin Cure, South Korea). After the supports had been carefully removed from the samples, all the samples were finished using silicon carbide grinding paper with ascending grit sizes (600, 800, 1000, and 1200) at 300 rpm under a water coolant for 30 s by the same clinician. All the samples were dried with dryer papers after being kept in a water bath at 37 °C for 24 h. The thickness of the samples was controlled with a digital caliper (Digimatic AOS, Mituyoto A. G., Japan)23.

Flexure strength measurements

Bar-shaped samples were 3D printed and conventional denture base referring to ISO 4049 (25 × 2 × 2 mm)4,11,26. A three-point bending test was performed using a universal testing machine (Shimadzu Co., Kyoto, Japan). The samples were fixed between two supports (20 mm span) and loaded at a crosshead speed of 0.5 mm/min until fracture occurred11.

Compressive strength measurements

The 30 samples in each group were subjected to compressive strength tests. The samples with a 6 mm diameter and 12 mm height were used as specified in the ISO 5833 standard27. The compressive strength tests were performed using a universal testing machine (Shimadzu Co., Kyoto, Japan) with a crosshead speed of 1 mm/min.

Vickers hardness measurements

The dimensions of the samples were 10 mm in diameter and 2 mm in thickness, and their surface microhardness was measured using a Vickers hardness testing device (Shimadzu HMV-G, Japan). The results were reported as the Vickers hardness number. Based on previous studies and the pilot study we conducted, a load of 50 N was applied for 10 s. The measurements were taken at three different points at a distance of at least 1 mm on each sample, and the mean values were recorded20.

Water absorption and solubility

All 30 samples of each test material were prepared with a diameter of 15 mm and a thickness of 1 mm (ISO 10477 1:2013)22,28. The upper and lower surfaces of the test samples were sanded with 600, 800, and 1000 grit silicon carbide (SiC) water abrasive (Struers GmbH). The samples were dried in a desiccator (POL-EKO-APARATURA, Wodzisław Śląski, Poland) that contained silica gel (Merck KGaA, Darmstadt, Germany) until a constant mass was reached. They were weighed daily on an analytical balance (OHAUS Corporation, New Jersey, USA) with an accuracy of 0.0001 g until a constant weight (m2) was reached. The samples were then placed in distilled water at 37 °C ± 1 °C and weighed regularly until a constant mass was reached. They were then removed from the water and returned to the desiccator. The drying procedure described above was repeated until a constant mass (m3) was reached12.

The water absorption (Wsp) and solubility (Wsl) values ​​for each sample (µg/mm3) were calculated using the following equations:

Inline graphic

where m1 is the constant mass before immersion in water (µg), m2 is the constant mass of the sample after immersion in water (µg), m3 is the constant mass after redrying (µg), and V is the volume of the sample (mm312.

Statistical analysis

The data were analyzed using IBM SPSS version 23. Normal distribution was assessed with the Shapiro–Wilk test. An independent sample t-test was used to compare the quantitative data that showed normal distribution for two-category independent variables, and the Mann–Whitney U test was used to compare the quantitative data that were not normally distributed. Multivariate Analysis of Variance (MANOVA) was used to compare multiple normally distributed quantitative variables across groups. Additionally, Pearson’s correlation and Spearman’s correlation were used to examine the relationships between quantitative variables. Mean ± standard deviation and median (min–max) were used to display the quantitative data. The significance level was established as p < 0.05.

Results

Mechanical tests

The mean values ​​for flexural and compressive strength and microhardness revealed statistically significant differences between the groups (p < 0.001). The mean flexural and compressive strength and microhardness values ​​of the 3D printed group were higher than those ​​of the conventional group (Table 2). The main effect of the material was found to be significant on flexural strength, compressive strength, and microhardness values (p < 0.001) (Table 3).

Table 2.

Comparison of mechanical properties according to groups.

3D printed (n = 30) Conventional (n = 30) Test statistic p*
Flexural strength 138.45 ± 7.48 111.02 ± 15.2 8.872 < 0.001
Microhardness 45.14 ± 7.65 25.49 ± 5.07 11.718 < 0.001
Compressive strength 106.37 ± 18.83 70.22 ± 6.81 9.887 < 0.001

*Independent sample t-test.

Significant values are in bold.

Table 3.

Multivariate analysis of variance (MANOVA) between mechanical parameters.

Mechanical parameters SS df MS Test statistic p η
Material Flexural strengtha 11286.896 1000 11286.896 78.707 < 0.001 0.576
Microhardnessb 5787.908 1000 5787.908 137.314 < 0.001 0.703
Compressive strengthc 19604.507 1000 19604.507 97.757 < 0.001 0.628

Significant values are in bold.

aR2: %57, 60.

bR2: %69, 80.

cR2:%62,10.

Water absorption and solubility

The mean water absorption value was lower in the 3D printed group compared to the conventional group, and the difference between these values ​​was statistically significant (p < 0.001). A statistically significant difference was obtained between the groups in terms of the water solubility values ​​(p = 0.003) (Table 4). In addition, the mean water absorption and water solubility values according to materials are illustrated in Figs. 1 and 2.

Table 4.

Comparison of water absorption and water solubility according to groups.

3D printed (n = 30) Conventional (n = 30) Test statistic p **
Water sorption 5.57 ± 1.09 10.53 ± 1.47 0.000 < 0.001
5.66 (2.26–7.36) 10.19 (8.49–15.85)
Solubility − 1.89 ± 2.2 − 3.28 ± 1.61
− 2.26 (− 6.23 to 5.1) − 3.67 (− 5.1 to 1.7) 248.000 0.003

**Mann Whitney U test.

Significant values are in bold.

Fig. 1.

Fig. 1

Water absorption values according to materials.

Fig. 2.

Fig. 2

Water solubility values according to materials.

In the 3D Printed group, a statistically significant, moderate negative correlation was found between microhardness and water solubility values (r = -0.483; p = 0.007). In the conventional group, a statistically significant, weak positive correlation was observed between water sorption and water solubility values (r = 0.398; p = 0.029).

As a result of the correlation analysis, regardless of the material type, strong positive correlations were identified among flexural strength, compressive strength, and microhardness. While water sorption exhibited a negative correlation with these mechanical properties, weaker but statistically significant correlations were found with water solubility (Table 5).

Table 5.

Correlation between quantitative variables.

Flexural strength Microhardness Compressive strength Water sorption
r p r p r p r p
3D printed
 Flexural strength
 Microhardness − 0.016x 0.933
 Compressive strength 0.263x 0.160 0.152x 0.424
 Water sorption 0.092y 0.629 − 0.057y 0.763 0.302y 0.105
 Solubility 0.053x 0.781 − 0.483x 0.007 − 0.265x 0.157 − 0.088y 0.646
Conventional
 Flexural strength
 Microhardness 0.323x 0.082
 Compressive strength 0.036x 0.850 0.086x 0.652
 Water sorption 0.223y 0.236 0.176y 0.353 0.071y 0.708
 Solubility − 0.060y 0.751 0.163y 0.390 0.065y 0.735 0.398y 0.029
Total
 Flexural strength
 Microhardness 0.715y < 0.001
 Compressive strength 0.671y < 0.001 0.767y < 0.001
 Water sorption − 0.619y < 0.001 − 0.734y < 0.001 − 0.687y < 0.001
 Solubility 0.311y 0.016 0.275y 0.033 0.280y 0.030 − 0.259y 0.046

xPearson korelasyon.

ySpearman’s rho korelasyon.

Significant values are in bold.

Discussion

In this in vitro study, we compared the mechanical properties water absorption and solubility of conventional and 3D-printed denture base materials. Statistically significant differences were found between the groups for all parameters, and the null hypothesis was rejected.

Volumetric and linear shrinkage is one of the structural characteristics of heat-cured resins. Digital processing techniques, however, almost completely eliminate this shrinkage. However, the main disadvantage of 3D printed denture bases is that they have a low double bond conversion rate compared to other types of acrylic resins. This can have a negative effect on their mechanical properties29. Due to the limited number of studies on the subject, definitive judgments cannot be made about the mechanical properties of 3D printed denture bases. Therefore, in this study, we compared the mechanical properties and water absorption and solubility of the denture base materials produced via 3D printing with those of the conventional denture base materials.

The mechanical properties of 3D printed resin are affected by production parameters, such as the printing angle, curing process, number of layers, and thickness. Acceptable layer thickness is generally determined as 100 µm11,21,23 and in this study, production was carried out with a layer thickness of 100 μm. The angle and structure of the layers can significantly affect the load-carrying capacity and general durability of the material. The literature shows that vertically positioned objects have higher compressive strength than horizontally positioned ones21,30. In this study, a 90° printing direction was preferred in the production of the 3D samples.

Flexural strength is a critical feature that directly affects the reliability, durability, and functionality of denture bases. Denture bases are constantly exposed to mechanical stresses in the mouth. During chewing, speaking, and oral movements, dentures are subjected to bending and twisting forces. Denture bases that do not have sufficiently high flexural strength are at risk of cracking or breaking under these forces29.

In studies in which the bending strength of 3D printed PMMA was compared with conventionally heat-polymerized PMMA, it was determined that the 3D printed PMMA bending strength value was lower than that of the conventionally produced PMMA16,21,25. In a meta-analysis comparing CAD/CAM, conventional, and 3D printed PMMA, the 3D printed PMMA was shown to have the lowest flexural strength of all the materials tested29. This low flexural strength value was attributed to the material’s low double bond conversion rate and poor adhesion between layers. In contrast, in the current study, we found that the fracture resistance of the 3D printed PMMA was higher than that of the conventionally produced PMMA.

Microhardness in denture base materials is an important parameter that is used to evaluate a material’s surface properties and the resistance of the material to mechanical forces applied to its surface. It indicates the resistance of the denture surface to scratches, abrasions, and deformation. Sufficient microhardness will ensure the longevity of the denture and increase the comfort of use of the patient. The microhardness properties of the materials used in the production of dentures are therefore a critical evaluation criterion for clinical success16. The higher microhardness value of the 3D printed group in this study suggests that the materials used may be more resistant to surface wear and provide longer term use. Harder surfaces also offer aesthetic and hygiene advantages by reducing plaque buildup and staining. The results of previous comparative studies showed that the hardness of 3D printed PMMA that was not subjected to thermal cycling was lower than that of heat-polymerized and milled CAD/CAM materials16,31. The decrease in hardness may have been due to the composition of the material, the printing layers, thermal stress, and water absorption. Another study had similar findings for 3D printed resin that was both thermally and nonthermally cycled21. The monomer conversion rate is an important indicator of the physical and mechanical properties of resin, and incomplete conversion can cause free monomers to remain in the final product and negatively affect the mechanical properties of the material. The most effective method to improve this situation is to increase the post-curing time. When previously examined, researchers noted that the post-curing time was limited to a maximum of 10 min29. Differences between studies can be attributed to variables such as the post-curing time and layer thickness.

The compressive strength of denture base material determines its resistance to high pressure, such as chewing forces, and ensures the dimensional stability, durability, and long-term use of the denture by reducing the risk of breakage. High compressive strength contributes to the denture maintaining its shape without deformation, increasing intraoral compliance, and ensuring clinical success32,33. In the present study, the average compressive strength value of the conventional PMMA was found to be consistent with that in the study of Shakir et al.33 At the same time, the average compressive strength value of the 3D printed group was significantly higher than that in the conventional group. However, this finding is not consistent with the results of the study by Arora et al.25 This difference could be attributed to the fact that in the latter study, the 3D printed samples were produced in a horizontal direction, and the postcuring time was limited to 10 min25. Indeed, Alharbi et al.34, showed in their study on 3D printed resin that the compressive strength of the material produced in a 90° printing direction was higher than that produced in a 0° printing direction.

Researchers who investigated the effects of the light-curing time on the physical–mechanical properties of 3D printed PMMA-based prosthetic material concluded that the 3D physical–mechanical properties improved with a postcuring time of 20 min23. Additionally, they found that the 3D printed prosthetic base material exhibited physical–mechanical properties similar to those of the conventional heat-cured group when postcured for 20 min.

In the present study, we determined that the 3D fabricated denture base was superior to the conventional one with respect to the mechanical parameters evaluated. This difference from previous studies could be attributed to the type of material used, the production angle, and the length of the post-curing period12.

The water absorption and solubility of the denture base material are critical to the mechanical strength, biological compatibility, dimensional stability, and aesthetic performance of the denture. High water absorption and solubility can reduce the strength of the material, lead to cracking and deformation, create hygiene problems due to microorganism accumulation, and increase the release of residual monomers, which can cause irritation in the oral tissues. In addition, this can impair the dimensional stability of the denture and negatively affect fit and comfort12,13,35.

In the current study, the water absorption value of the conventional denture base material was found to be higher than that of the 3D printed denture base. Contrary to our study, there are studies in the literature in which the water absorption value of the conventional PMMA material was lower than that of the 3D printed denture base13,36,37. In one study, the 3D printed materials showed a similar water absorption tendency to the conventional materials22. These differences in results can be attributed to the chemistry of the materials used and differences in the postcuring methods and times as well as the layer thickness used in production. An increased amount of layering may be a reason for the increased water absorption. The absorbed water enters between the layers, and the water molecules then diffuse into the polymers of the resin, which allows the interpolymer spaces to be filled with water, thereby displacing the polymer chains from the other chains13,36. In another study, the researchers found that 3D printed PMMAs have higher water absorption compared to conventional PMMAs37. They also evaluated the effect of the printing angle used when producing 3D printed PMMA on the physical properties of the material. According to the results, the printing angle significantly affected water absorption and solubility. A decrease in water absorption was observed as the printing angle increased from 0° to 90°. The 90° printing angle, 100 μm layer thickness, and 30 min postcuring time used in the current study explain our results.

In our study, the water solubility values ​​of both groups showed negative values. The water solubility values ​​of PMMA were also measured as negative in the studies conducted by Tuna et al.35 and Nguyen et al.12 The researchers concluded that the tested materials were chemically bonded with water molecules and thus could not absorb and release water.

In our study, the 3D printed denture base materials showed superior performance compared to the conventional materials in terms of mechanical properties and water absorption and solubility. This indicates that 3D printing technology can provide more durable and long-lasting materials in prosthesis production.

This study has some limitations. First of all, only one 3D printer model and one PMMA material were used, and no variation was applied in the printing parameters. In addition, the study only evaluated the mechanical properties and biological or microbiological properties were not examined. In addition, the study was completely conducted in vitro, and clinical simulations such as thermal cycling procedures and aging tests in artificial saliva were not included.

Conclusions

The denture base materials produced via the 3D printing method in our study exhibited a higher mechanical performance compared to those produced using a conventional method. In addition, the materials produced by 3D printing showed lower water absorption values ​​compared to the conventional group. Low water absorption rate improves biocompatibility by increasing the long-term stability of the material and contributes to maintaining the dimensional stability of the prosthesis in the oral environment. These results support the wider use of 3D printing technology in clinical applications in dentistry and show that it has the potential to improve patient comfort. Future studies should more comprehensively evaluate the effects of 3D printed denture bases on patient satisfaction, long-term biomechanical performance and the adaptation process. In particular, research integrating subjective feedback based on patient experiences and clinical observations will contribute to a better understanding of the effectiveness of this technology in dentistry.

Author contributions

Study design: Z.Ö. and B.T. Experimental and data analysis: Z.Ö. and B.T. Drafed the manuscript: Z.Ö. Reviewed the manuscript: Z.Ö. and B.T.

Data availability

The data will be made available by the corresponding author upon reasonable request.

Declarations

Competing interests

The authors declare no competing interests.

Footnotes

Publisher’s note

Springer Nature remains neutral with regard to jurisdictional claims in published maps and institutional affiliations.

References

  • 1.Aktaş, N. & Ciftci, V. Current applications of three-dimensional (3D) printing in pediatric dentistry: a literature review. J. Clin. Pediatr. Dent.48, 4–13 (2024). [DOI] [PubMed] [Google Scholar]
  • 2.Aydın, L. & Küçük, S. Üç Boyutlu Yazıcı ve Tarayıcı Ile Hastaya Özel medikal Ortez Tasarımı ve geliştirilmesi design and construction of ankle foot orthosis by means of three dimensional printers. Politek Derg. 20, 1–8 (2017). [Google Scholar]
  • 3.Wuersching, S. N., Hickel, R., Edelhoff, D. & Kollmuss, M. Initial biocompatibility of novel resins for 3D printed fixed dental prostheses. Dent. Mater.38, 1587–1597 (2022). [DOI] [PubMed] [Google Scholar]
  • 4.Borella, P. et al. Physical and mechanical properties of four 3D-printed resins at two different Thick layers: an in vitro comparative study. Dent. Mater.39, 686 (2023). [DOI] [PubMed] [Google Scholar]
  • 5.Yanar, G., İnal, C. & Aktaş, N. Bankoğlu Güngör, M. A severely damaged premolar tooth restored with coronal pulpotomy and a 3D-printed endocrown. J. Clin. Pediatr. Dent.48, 193–199 (2024). [DOI] [PubMed] [Google Scholar]
  • 6.Habib, A. A. I. & Sheikh, N. A. 3D printing review in numerous applications for dentistry. J. Inst. Eng. Ser. C. 103, 991–1000 (2022). [Google Scholar]
  • 7.Kharat, S. et al. Exploring the impact of 3D printing technology on Patient-Specific prosthodontic rehabilitation: A comparative study. J. Pharm. Bioallied Sci.16, 423–426. 10.4103/jpbs.jpbs_643_23 (2024). [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 8.Nabil, M. S., Mahanna, F. F. & Said, M. M. Evaluation of masticatory performance and patient satisfaction for conventional and 3D-printed implant overdentures: a randomized crossover study. BMC Oral Health. 24, 1–9 (2024). [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 9.Alqutaibi, A. Y. et al. Polymeric denture base materials: A review. Polym. (Basel)15, (2023). [DOI] [PMC free article] [PubMed]
  • 10.de Limírio, O. Mechanical properties of polymethyl methacrylate as a denture base: conventional versus CAD-CAM resin - A systematic review and meta-analysis of in vitro studies. J. Prosthet. Dent.128, 1221–1229 (2022). [DOI] [PubMed] [Google Scholar]
  • 11.Alshamrani, A. A., Raju, R. & Ellakwa, A. Effect of Printing Layer Thickness and Postprinting Conditions on the Flexural Strength and Hardness of a 3D-Printed Resin. Biomed Res. Int. (2022). (2022). [DOI] [PMC free article] [PubMed]
  • 12.Nguyen, L. G., Kopperud, H. M. & Øilo, M. Water sorption and solubility of polyamide denture base materials. Acta Biomater. Odontol. Scand.3, 47–52 (2017). [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 13.Gad, M. M. et al. Water sorption, solubility, and translucency of 3D-Printed denture base resins. Dent. J.10, (2022). [DOI] [PMC free article] [PubMed]
  • 14.Khan, A. A. et al. Mechanical properties of the modified denture base materials and polymerization methods: A systematic review. Int. J. Mol. Sci.23, 1–13 (2022). [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 15.Issa Salih, S. Investigation of fatigue and compression strength for the PMMA reinforced by different system for denture applications. Int. J. Biomed. Mater. Res.3, 5 (2015). [Google Scholar]
  • 16.Prpić, V., Schauperl, Z., Ćatić, A., Dulčić, N. & Čimić, S. Comparison of mechanical properties of 3D-Printed, CAD/CAM, and conventional denture base materials. J. Prosthodont.29, 524–528 (2020). [DOI] [PubMed] [Google Scholar]
  • 17.Naji, S. A. et al. Effects of incorporation of 2.5 and 5 Wt% TiO2 nanotubes on fracture toughness, flexural strength, and microhardness of denture base Poly Methyl methacrylate (PMMA). J. Adv. Prosthodont.10, 113–121 (2018). [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 18.Kim, M. C. et al. Color stability, surface, and physicochemical properties of three-dimensional printed denture base resin reinforced with different nanofillers. Sci. Rep.14, 1–12 (2024). [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 19.Altarazi, A., Haider, J., Alhotan, A., Silikas, N. & Devlin, H. Impact of Artificial Aging on the Physical and Mechanical Characteristics of Denture Base Materials Fabricated via 3D Printing. Int. J. Biomater. (2024). (2024). [DOI] [PMC free article] [PubMed]
  • 20.Alshaikh, A. A. et al. 3D-Printed Nanocomposite Denture-Base Resins: Effect of ZrO2 Nanoparticles on the Mechanical and Surface Properties In Vitro. Nanomaterials 12, (2022). [DOI] [PMC free article] [PubMed]
  • 21.Gad, M. M. et al. Strength and surface properties of a 3D-Printed denture base polymer. J. Prosthodont.31, 412–418 (2022). [DOI] [PubMed] [Google Scholar]
  • 22.Perea-Lowery, L., Gibreel, M., Vallittu, P. K. & Lassila, L. V. 3d-printed vs. Heat-polymerizing and autopolymerizing denture base acrylic resins. Mater. (Basel). 14, 1–11 (2021). [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 23.Aati, S. et al. Effect of post-curing light exposure time on the physico-mechanical properties and cytotoxicity of 3D-printed denture base material. Dent. Mater.38, 57–67 (2022). [DOI] [PubMed] [Google Scholar]
  • 24.Li, P., Lambart, A., Stawarczyk, B., Reymus, M. & Spintzyk, S. Postpolymerization of a 3D-printed denture base polymer: impact of post-curing methods on surface characteristics, flexural strength, and cytotoxicity. J. Dent.115, 103856 (2021). [DOI] [PubMed] [Google Scholar]
  • 25.Arora, O., Ahmed, N., Nallaswamy, D., Ganapathy, D. & Srinivasan, M. Denture base materials: an in vitro evaluation of the mechanical and color properties. J. Dent.145, 104993 (2024). [DOI] [PubMed] [Google Scholar]
  • 26.Tahayeri, Anthony, M. M. et al. 3D printed versus conventionally cured provisional crown and Bridge dental materials. Dent. Mater.34, 192–200 (2018). [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 27.International Standards Organization (ISO). ISO 5833: Implants for surgery-Acrylic Resin Cements (ISO, 2012).
  • 28.International Organization for Standardization (ISO). Dentistry—Base Polymers—Part 1: Denture Base Polymers; ISO 20795- 1:2013; International Organization of Standardization (ISO) (Geneva, 2013).
  • 29.Abualsaud, R. & Gad, M. Flexural strength of CAD/CAM denture base materials: systematic review and Meta-analysis of In-vitro studies. J. Int. Soc. Prev. Community Dent.12, 160–170 (2022). [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 30.Lyu, Q., Dai, P. & Chen, A. Mechanical strengths and optical properties of translucent concrete manufactured by mortar-extrusion 3D printing with polymethyl methacrylate (PMMA) fibers. Compos. Part. B Eng.268, (2024).
  • 31.Htat, H. L., Prawatvatchara, W., Techapiroontong, S., Lee, J. H. & Limpuangthip, N. Effect of mechanical and chemical surface treatments on the repairing of milled and 3D-printed denture bases. Sci. Rep.14, 1–10 (2024). [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 32.Aldegheishem, A., Aldeeb, M., Al-Ahdal, K., Helmi, M. & Alsagob, E. I. Influence of reinforcing agents on the mechanical properties of denture base resin: A systematic review. Polym. (Basel). 13, 1–12 (2021). [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 33.R, S. A., Selvi, K., Shankar, B., Hariharan, A. & S. S. & Comparative analysis of strength of differently activated denture base materials including recent acetal Resin-Based Biodentaplast. Cureus16, 1–10 (2024). [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 34.Alharbi, N., Osman, R. & Wismeijer, D. Factors influencing the dimensional accuracy of 3D-Printed Full-Coverage dental restorations using stereolithography technology. Int. J. Prosthodont.29, 503–510 (2016). [DOI] [PubMed] [Google Scholar]
  • 35.Tuna, S. H., Keyf, F., Gumus, H. O. & Uzun, C. The evaluation of water sorption/solubility on various acrylic resins. Eur. J. Dent.02, 191–197 (2008). [PMC free article] [PubMed] [Google Scholar]
  • 36.Dimitrova, M. et al. Evaluation of water sorption and solubility of 3D-Printed, CAD/CAM milled, and PMMA denture base materials subjected to artificial aging. J. Compos. Sci.7, (2023).
  • 37.Gulver, G. & Meric, G. Water sorption and solubility of 3D printed denture resin. Int. Dent. J.74, 10 (2024). [Google Scholar]

Associated Data

This section collects any data citations, data availability statements, or supplementary materials included in this article.

Data Availability Statement

The data will be made available by the corresponding author upon reasonable request.


Articles from Scientific Reports are provided here courtesy of Nature Publishing Group

RESOURCES