Abstract
Hydrogels are routinely used as scaffolds to mimic the extracellular matrix for tissue engineering. However, common strategies to covalently crosslink hydrogels employ reaction conditions with potential off-target biological reactivity. The limited number of suitable bioorthogonal chemistries for hydrogel crosslinking restricts how many material properties can be independently addressed to control cell fate. To expand the bioorthogonal toolkit available for hydrogel crosslinking, we identify isonitrile ligations as a promising class of reactions. Isonitriles are compact, stable, selective, and biocompatible moieties that react with chlorooxime (ChO), tetrazine (Tz), and azomethine imine (AMI) functional groups under physiological conditions. We demonstrate that all three ligation reactions can form hydrogels, with isonitrile-ChO ligation exhibiting optimal gelation properties. Synthetic poly(ethylene glycol) (PEG) hydrogels crosslinked by isonitrile-ChO ligation exhibit rapid gelation kinetics, elastic mechanical properties, stability under physiological conditions, and high biocompatibility. By combining ChO-functionalized multi-arm PEGs with isonitrile-functionalized engineered elastin-like proteins (ELPs), we demonstrate simultaneous control over network connectivity and adhesive ligand presentation, which in turn regulate cell spreading. These hydrogels enable the long-term culture of numerous human cell types relevant to regenerative medicine. Furthermore, we demonstrate that isonitrile-ChO ligation is orthogonal to common azide-alkyne cycloaddition, enabling independent, bioorthogonal functionalization of hydrogels containing live cells.
Keywords: isonitrile ligation, engineered extracellular matrices, recombinant protein materials, hydrogels, bioorthogonal chemistry
Graphical Abstract

Highly selective chemistries are required for fabrication and post-crosslinking modification of cell-encapsulating hydrogels used in tissue engineering applications. Isonitrile ligation reactions represent a promising class of bioorthogonal chemistries for engineering hydrogel-based cellular microenvironments. Isonitrile-based hydrogels are stable, cytocompatible, and enable precise chemical functionalization in the presence of live cells.
1. Introduction
Hydrogels are often applied as tissue engineering scaffolds to mimic the extracellular matrix (ECM) due to their high-water content, comparable mechanical properties to native tissues, biocompatibility, and ability to present bioactive cues to cells.[1] The biochemical and mechanical properties of hydrogels regulate cell adhesion, spreading, proliferation, and other aspects of cell fate.[2] Therefore, independent tuning of hydrogel properties is required to optimally control the function of cells within these materials. To achieve decoupled control of material properties, the use of mutually orthogonal chemistries is necessary. Further, ideal chemistries would not cross-react with biological functional groups that could unintentionally disrupt cell function; that is, the chemistries should also be bioorthogonal. At present, the most common chemistries used to prepare cell encapsulating hydrogels can react with functional groups present on cells, such as thiols or amines, or make use of free radical mediated reactions, which may damage sensitive primary cells or stem cell-derived cells used in regenerative medicine applications. To date, only two bioorthogonal chemistries possess sufficient chemical selectivity to avoid cross-reactivity with live cells while having sufficiently rapid reaction kinetics to form hydrogels: strain-promoted azide-alkyne cycloaddition (SPAAC) and tetrazine-mediated inverse electron demand Diels-Alder (IEDDA) reactions. Given the relatively bulky and hydrophobic nature of the tetrazine-reactive dienophiles used in IEDDA reactions, we set out to identify alternative bioorthogonal reactive partners that were compact and stable, causing minimal perturbations to the biological system, similar to azides used in SPAAC. Isonitriles (NC), also known as isocyanides, are comprised of only two atoms and rarely occur in biological contexts,[3] making them ideal as potential reactive partners in bioorthogonal functionalization of cell encapsulating hydrogels.
In organic chemistry, isonitriles have proven to be versatile functional groups, serving as electrophiles, nucleophiles, and metal coordination ligands.[4] Because of their small size, favorable solubility, lack of biological cross-reactivity, and stability under physiological conditions, isonitriles can be incorporated into biological systems with minimal perturbation.[5] Multiple isonitrile-based ligations, including those with tetrazines (Tz), azomethine imines (AMI), and chlorooximes (ChO), have been applied in identifying natural compounds,[6] labelling peptides and proteins,[7] and releasing drug payloads.[8] The isonitrile-tetrazine reaction is the most extensively studied of these ligation reactions. Tetrazines react with isonitriles via bioorthogonal cycloaddition to afford imine linked products. Azomethine imines react selectively with isonitriles in the presence of biological function groups to obtain acyl amide ligation products. Recently, the isonitrile-AMI ligation reaction was applied to label proteins on the surface of live cells, demonstrating excellent biocompatibility.[9] Chlorooximes decompose to highly reactive nitrile oxides in aqueous conditions and subsequently react with isonitriles to form stable hydroxyamino amide adducts.[10] Importantly, isonitrile-ChO ligation could proceed selectively without disturbing native biochemistry, and has been used in labelling, detection, isolation and structural elucidation of isonitrile-containing natural products.[6a, 7a]
Consistent with their reported role as bioorthogonal reactions, isonitrile-based ligations do not require toxic catalysts, UV light irradiation, or highly unstable reaction partners. Isonitriles are underutilized functional handles that exhibit exquisite chemoselectivity, fast reaction rates, low cytotoxicity, and compatibility with other reactions in cellular systems. Furthermore, isonitrile ligations can be designed to be orthogonal to SPAAC-based bioorthogonal reactions, highlighting their potential use to independently modify cellular microenvironments using two separate bioorthogonal reactions. Given the favorable reaction rates, versatility, and biorthogonality of isonitrile-mediated ligations, we envisioned that hydrogel materials crosslinked by isonitrile ligations could be used to precisely control the physical and chemical properties of 3D cellular environments. We designed polyethylene glycol (PEG) and recombinant elastin-like protein (ELP) based hydrogels employing isonitrile ligation reactions to facilitate crosslinking and subsequent chemical modification. The resulting hydrogels demonstrated tunable elasticity, excellent cytocompatibility, and the ability to regulate cell adhesion and spreading in 3D. Moreover, isonitrile-based ligations were shown to be mutually orthogonal to current bioorthogonal hydrogel modification strategies that employ SPAAC. Our findings indicate that isonitriles present a promising strategic functional group for the design of biomaterials with applications in tissue engineering and regenerative medicine.
2. Results
2.1. Isonitrile-chlorooxime ligation exhibits optimal gelation properties
To determine whether the three known bioorthogonal isonitrile ligations were suitable for crosslinking reactions to form cell encapsulating hydrogels, we first sought to form synthetic hydrogels from multi-arm PEGs modified with isonitriles and either chlorooximes, azomethine imines, or tetrazines. The isonitrile-containing precursor, perfluorophenyl 3-isocyanopropanoate, was prepared according to published protocols[11] and reacted with 8-arm PEG-amine to afford 8-arm PEG-isonitrile (PEG-NC). Eight-arm PEGs functionalized with chlorooximes (PEG-ChO), azomethine imines (PEG-AMI), and tetrazines (PEG-Tz) were similarly prepared from 8-arm PEGs, adapting known synthetic routes.[12] Eight-arm PEGs were chosen as the high degree of macromer functionality results in a lower percolation threshold for gelation, thereby decreasing the time to reach the gel point. The molecular weight was kept constant at 20 kDa to provide sufficient arm length to maintain flexibility in the network and minimize defect formation. The isonitrile functionalized-PEGs react with PEG-ChO, PEG-AMI, and PEG-Tz to obtain hydrogel networks comprised of hydroxyamino amide, acyl amide, and imine ligation products, respectively (Figure 1A,B). Oscillatory rheology was performed to measure the gelation kinetics of hydrogels crosslinked by the three isonitrile ligations. Based on a preliminary screen of polymer concentrations, all formulations used in these experiments contained 5% (w/v) PEG dissolved in phosphate-buffered saline (PBS), which yielded hydrogels with physiologically-relevant storage moduli (G’~103 Pa). The gelation time was defined as the point at which the storage modulus (G’) first exceeded the loss modulus (G”) under conditions of 5% strain and 1 Hz oscillatory frequency. The isonitrile-ChO gels exhibited the most rapid gelation kinetics, reaching the gel point in less than five minutes at 22 °C and pH 7.4 (Figure 1C,D). Increasing the reaction temperature to 37 °C was required to accelerate the isonitrile-AMI and isonitrile-Tz crosslinking reactions, which still afforded relatively slow gelation times that were significantly longer than that of the isonitrile-ChO gels (Figure 1C,D).
Figure 1.

Isonitrile-based ligations for bioorthogonal crosslinking of cell-encapsulating hydrogels. (A) Reaction schemes for isonitrile-ChO, -AMI, and -Tz ligations. (B) Idealized schematic depicting formation of 8-arm PEG isonitrile-based hydrogels. (C) Gelation time sweep showing storage moduli of 5% (w/v) 8-arm PEG isonitrile-ChO, -AMI, and -Tz hydrogels crosslinked at 22 °C, 37 °C, and 37 °C, respectively. (D) Gelation time for and (E) plateau storage moduli (G’) of 5% (w/v) 8-arm PEG isonitrile-ChO, -AMI, and -Tz hydrogels crosslinked at 22 °C, 37 °C and 37 °C, respectively. (F) Mass swelling ratio as a function of time for 5% (w/v) 8-arm PEG isonitrile-ChO, -AMI, and -Tz hydrogels over time for samples maintained in complete cell culture medium (DMEM + 10% FBS) at 37 °C. (G) Photograph of 8-arm PEG isonitrile-ChO, -AMI, and -Tz hydrogels. (H) Fluorescence micrographs and quantification of cell viability after 1 hour of culture for live/dead-stained human fibroblasts encapsulated in isonitrile-ChO hydrogels at pH 7.4 and 5% (w/v) polymer content (left) and isonitrile-AMI hydrogels at pH 6 and 5% (w/v) polymer content (right). Green: live (calcein-AM), red: dead (ethidium homodimer). In D-F, data are presented as mean ± s.d., n = 3. ***p<0.001, ****p<0.0001, one-way ANOVA with Bonferroni post-hoc test.
While the gelation kinetics for the isonitrile-ChO gels were more favorable, the storage moduli of the resulting gels were significantly less than those for the AMI and Tz-based gels. We hypothesized that the faster gelation kinetics of the isonitrile-ChO reaction resulted in a greater concentration of network defects. The potential for defects would be expected to increase as the reaction rate increases.[13] Thus, we assessed whether increasing the gelation temperature to 37 °C would further increase the gelation rate and decrease the storage modulus. Indeed, when gelled at 37 °C, both the gelation time and the storage modulus of the gels significantly decreased (Figure S1A,B, Supporting Information). While reducing the gelation temperature to 4 °C did further reduce the speed of gelation, the storage modulus was comparable to the gels prepared at 22 °C (Figure S1A,B, Supporting Information). Thus, there appears to be some basal level of defects that are exacerbated by faster gelation. If the decrease in modulus upon changing the gelation temperature from 22 °C to 37 °C is due to increased defects in the gels prepared at 37 °C, then we would expect to see both unreacted isonitrile and ChO groups. To assess whether more unreacted isonitrile groups remained in gels prepared at 37 °C compared to those prepared at 22 °C, the gels were characterized by FTIR (Figure S2, Supporting Information). As illustrated by comparing unreacted PEG-NC with unreacted PEG-ChO, the observed peak at 2153 cm−1 can be attributed to the isonitrile stretch vibration.[14] In contrast to gels prepared at 22 °C, a clear peak remained around 2152 cm−1 in gels prepared at 37 °C, indicating the presence of residual unreacted isonitrile groups. One competing mechanism for the increase of defects in the network would be increased decomposition of the nitrile oxide intermediates generated from the ChO during crosslinking at higher temperatures. To determine whether residual nitrile oxide groups remained following crosslinking, hydrogels prepared at 22 °C or 37 °C were reacted with a norbornene-PEG6-pyrene dye.[12a] Significantly greater fluorescence intensity was measured in gels prepared at 37 °C compared to 22 °C (Figure S3, Supporting Information). Thus, even when gelation was complete, as indicated by the storage moduli reaching a stable plateau, higher concentrations of both isonitrile and ChO-derived reactive groups were present in gels prepared at 37 °C, suggesting increased defect formation was due to faster reaction rates with increasing temperature. Thus, in subsequent experiments, gelation of isonitrile-ChO gels was performed at 22 °C.
The isonitrile-AMI reaction is pH sensitive,[9] so we further investigated whether decreasing the pH of the gelation buffer would accelerate the crosslinking of isonitrile-AMI gels. Solutions of 8-arm PEG-NC and 8-arm PEG-AMI, both at 5% (w/v), were prepared in PBS with pH adjusted to 6, 6.5, and 7, and compared to the standard formulation of PBS at pH 7.4. Hydrogels formed by mixing these solutions in 3:2 volumetric ratios at 37 °C were assessed by oscillatory rheology. As anticipated, decreasing the pH resulted in faster gelation (Figure S4A, Supporting Information). However, similar to the isonitrile-ChO gels, increasing the gelation rate of the isonitrile-AMI gels resulted in decreased storage moduli (Figure S4B, Supporting Information). We likewise attribute this drop in modulus to increases in network defects due to more rapid crosslinking, as performing the gelation at 22 °C and pH 6 gave slower kinetics and higher storage moduli (Figure S4A,B, Supporting Information). Thus, the gelation rate of the isonitrile-AMI gels can be increased by decreasing the pH of the crosslinking solution.
To use isonitrile ligation-based gels as tissue engineering scaffolds, the resulting crosslinks should be stable to hydrolysis and enzymatic degradation to prevent rapid gel swelling and degradation in cell culture environments. While the hydroxyamino amide and acyl amide linkages resulting from isonitrile ligation with ChO and AMI groups, respectively, are expected to be stable, the imine groups generated in Tz-based ligations are often chosen because of their ability to rapidly hydrolyze. The propanoate isonitrile linker we used was previously shown to resist hydrolysis,[15] indicating the linkages in our system may be more stable. Hydrogels prepared by the three ligation methods were maintained in either PBS or complete cell culture medium (Dulbecco’s modified Eagle medium (DMEM) plus 10% fetal bovine serum (FBS)) at 37 °C, and degradation was monitored by measuring the mass swelling ratio and the dry mass of PEG remaining over the course of 14 days. All three formulations demonstrated good stability, showing no substantial changes in swelling (Figure 1F; Figure S5, Supporting Information) or mass loss (Figure S6–7, Supporting Information), indicating that the crosslinks resist hydrolysis as well as degradation by serum enzymes. To use the isonitrile groups as bioorthogonal reactive handles for subsequent gel modification, unreacted isonitriles must also remain stable under cell culture conditions. Isonitrile-ChO crosslinked PEG gels maintained in complete culture medium were dried and characterized by FTIR. The resulting spectra exhibited clear isonitrile stretch vibration peaks around 2150 cm−1 that were stable over the course of 14 days (Figure S8, Supporting Information). Collectively, these results demonstrated that PEG based hydrogels are stable in vitro.
One additional difference among the three ligation reactions is that the Tz-based ligations produce nitrogen gas as a byproduct. While benign to cells, the gas production resulted in the formation and trapping of bubbles within the gels during crosslinking (Figure 1G). Bubble formation was not observed in the ChO- or AMI-based ligation gels. Thus, we concluded that isonitrile-Tz ligations were not suitable for formation of cell-encapsulating hydrogels as the primary crosslinking method.
To determine whether the optimized gelation conditions (Table 1) for isonitrile-ChO and isonitrile-AMI gels were cytocompatible, MRC5 human fetal lung fibroblasts were encapsulated in 5% (w/v) 8-arm PEG hydrogels at a density of 106 cells/mL. Isonitrile-ChO gels were prepared by reacting at room temperature for 10 min and then moving to the cell culture incubator for another 20 min to complete crosslinking. Isonitrile-AMI gels were prepared by immediately transferring to the incubator to accelerate crosslinking. The acute viability of the fibroblasts was measured after 1 hour in culture by live/dead staining to assess any fast-acting toxic effects of crosslinking, following our published procedures.[2b] In both the ChO- and AMI-based gels, the cells remained highly viable (>95% live) (Figure 1H). Thus, both isonitrile-ChO and isonitrile-AMI ligations are cytocompatible crosslinking reactions, as the lower pH of the AMI buffers did not result in appreciable cell death (Figure 1H; Figure S4C, Supporting Information). Nevertheless, because the lower pH may otherwise impact cell fate, we selected the isonitrile-ChO ligation reaction to further investigate the use of isonitriles as bioorthogonal chemical handles to engineer extracellular environments.
Table 1.
Optimal gelation conditions for PEG-isonitrile crosslinking with ChO, or AMI, or Tz functionalized PEGs
| Ligation | Temperature [°C] | pH | Gelation Time [s]a) | Modulus (G’) [Pa] | Side Product | Note |
|---|---|---|---|---|---|---|
| Isonitrile-ChO | 22 | 7.4 | 280 ± 10 | 1833 ± 247 | HCl | Increasing temperature increases defects |
| Isonitrile-AMI | 22 | 6 | 430 ± 13 | 6809 ± 1129 | None | Acidic pH required to accelerate crosslinking |
| 37 | 6 | 132 ± 8 | 3206 ± 713 | None | Increased temperature increases defects | |
| Isonitrile-Tz | 37 | 7.4 | 638 ± 34 | 5006 ± 202 | N2 | Gas bubbles are trapped in gels during crosslinking |
Time at which the storage modulus first exceeded the loss modulus.
2.2. Isonitrile-ChO hydrogels exhibit tunable elasticity
The mechanical properties of the cellular microenvironment are critical regulators of cell fate.[16] Thus, any hydrogel scaffold used for tissue engineering applications should enable precise control over the mechanical properties of the material. To demonstrate that isonitrile-ChO hydrogels exhibit tunable elastic properties, rheological testing was performed for hydrogels with polymer content ranging from 5% to 10% (w/v). 8-arm PEG-NC was crosslinked with 8-arm PEG-ChO in PBS at 22 °C to form hydrogels that were subjected to 5% strain at 1 Hz oscillatory frequency (Figure 2A). As expected for increasing polymer and reactive group concentrations, the gelation time decreased as the PEG concentration increased (Figure 2B; Figure S9, Supporting Information). The plateau storage moduli (G’) increased as the polymer content increased, confirming that the stiffness of the hydrogels could be tuned over a physiologically relevant range (G’~1–10 kPa) (Figure 2C). As time-dependent, viscoelastic cues are also known to impact cell fate,[1a, 16c] we also investigated the frequency- and strain-dependent behavior of the isonitrile-ChO PEG networks. Frequency sweeps at a fixed 5% strain revealed that G’ and G” remained consistent as frequency was varied from 0.1 to 10 Hz (Figure 2D). Similarly, strain sweeps revealed consistent moduli values across 0.1 to 10% strain (Figure 2E). Furthermore, across both frequency and strain sweeps, G’ was much greater than G”. Taken together, these results indicate that PEG isonitrile-ChO hydrogels behaved as predominantly elastic materials with tunable stiffness.
Figure 2.

Isonitrile-ChO hydrogels behave as predominantly elastic materials. (A) Gelation time sweeps, (B) gelation times, (C) plateau storage moduli (G’), (D) frequency sweeps at 5% strain, and (E) strain sweeps at 1 Hz oscillatory frequency for 8-arm PEG isonitrile-ChO hydrogels with polymer contents of 5%, 6%, 7.5%, and 10% (w/v). In B and C, data are presented as mean ± s.d., n = 3.
2.3. Independent tuning of network connectivity and adhesive ligand presentation regulates cell spreading in 3D
As PEG is not inherently bioactive, we next investigated whether engineered elastin-like proteins (ELPs) could be functionalized with isonitriles to incorporate cell adhesion and proteolytic degradation motifs into isonitrile-ChO hydrogels.[17] The small size and good solubility of isonitriles suggested that they should be able to be incorporated into ELPs without detrimentally impacting protein solubility. The ELPs used in this study contain either a cell-adhesive RGD sequence derived from human fibronectin or a scrambled, non-adhesive RDG sequence.[18] To decouple the crosslinking of the hydrogels from the cell adhesion domain, the structural domain of these ELPs was comprised of VPGXG elastin-like repeats in which 1 out of 5 X amino acid residues was a lysine to provide a primary amine for chemical modification (Figure 3A). The remaining X residues were non-reactive isoleucines. Protein purity was confirmed by sodium dodecyl sulfate-polyacrylamide gel electrophoresis (SDS-PAGE) (Figure S10, Supporting Information). Isonitrile functionalized ELPs were synthesized by reacting the free amines on the ELP with perfluorophenyl 3-isocyanopropanoate. 1H NMR analysis suggested that the ELP was fully functionalized with isonitriles, based on the disappearance of the peak corresponding to the ε-protons of lysines with free primary amines (Figure S11, Supporting Information).
Figure 3.

Independent tuning of network connectivity and adhesive ligand content regulates cell spreading in 3D. (A) Schematic illustration of RGD-containing, isonitrile-functionalized ELPs crosslinked with PEG-bis-ChO to form hydrogel networks. (B) The storage moduli (G’) of isonitrile-ChO ELP-PEG hydrogels were maintained consistent regardless of network connectivity and adhesive ligand presentation. (C) The gelation time of isonitrile-ChO ELP-PEG hydrogels decreases with increasing crosslinker functionality but does not vary with adhesive ligand presentation. (D) Quantification of cell spread area for fibroblasts encapsulated in isonitrile-ChO ELP-PEG hydrogels after 7 d, calculated from maximum intensity projections of phalloidin staining. (E) Representative confocal micrographs of cell spreading in isonitrile-ChO ELP-PEG hydrogels. In B-D, data are presented as mean ± s.d., n = 3. n.s. = not significant (p>0.05), *p<0.05, **p<0.01, ***p<0.001, ****p<0.0001, one-way ANOVA with Bonferroni post-hoc test.
The control over macromolecular architecture afforded by the ELPs and the multi-arm PEGs combined with the chemical selectivity of the isonitrile ligation reaction allows for decoupled control over two hydrogel properties known to regulate cell behavior in 3D: hydrogel network connectivity and cell adhesive ligand presentation. To be able to spread in 3D, cells need to both remodel the surrounding material through proteolytic degradation and adhere to the material via cell surface receptors such as integrins. We previously demonstrated that remodelability of ELP-PEG hybrid hydrogels can be tuned by altering the functionality of the PEG crosslinkers, with bis-functionalized PEGs permitting extensive remodeling and spreading and 8-arm PEGs largely blocking remodeling.[17] We thus prepared a series of PEG-ChO with different functionalities, including PEG-bis-ChO, 3-arm PEG-ChO, and 8-arm PEG-ChO. The PEG-ChO crosslinkers were mixed with isonitrile-functionalized ELPs to generate hydrogels (Figure 3A; Figure S12–13, Supporting Information). As the stiffness of the hydrogel network and the concentration of RGD adhesive ligands has also been shown to regulate cell spreading in 3D ELP systems,[2b] the polymer content of the hydrogels was tuned within a narrow range to ensure that network connectivity and the presence of RGD adhesive ligands were the only variables being tested (Figure S14–16, Supporting Information). The resulting gel formulations exhibited similar storage moduli of ~2 kPa (Figure 3B), which is within a physiologically relevant stiffness range previously shown to support cell spreading in 3D.[2b] As expected, the materials comprised with higher functionality crosslinkers exhibited faster gelation kinetics (Figure 3C), as these materials have a lower percolation threshold to achieve gelation.[17]
To demonstrate that the independent control over network connectivity and adhesive ligand concentration in this system can regulate cell phenotype, MRC5 fibroblasts were encapsulated within hydrogels of varying crosslinker functionality and RGD ligand presentation and cultured for 7 days to permit proteolytic remodeling of the materials. To assess cell spreading, the fibroblasts were subsequently fixed, stained with phalloidin-tetramethylrhodamine B isothiocyanate to label the actin cytoskeleton, and imaged by laser scanning confocal microscopy. Cell spread area was calculated from maximum intensity projections. In hydrogels containing RGD adhesion ligands, extensive cell spreading was observed in the bis-functionalized crosslinker gels, more limited spreading in the 3-arm crosslinker gels, and minimal spreading in the 8-arm crosslinker gels (Figure 3D,E). Qualitatively, the cell morphologies were distinct in these three crosslinker conditions, with cells cultured in bis-functionalized PEG gels exhibiting highly elongated morphologies, cells cultured in 3-arm PEG gels exhibiting a series of smaller protrusions, and cells cultured in 8-arm PEG gels remaining largely rounded (Figure 3E). Demonstrating decoupled control of network connectivity and adhesive ligand concentration, cells cultured in bis-functional PEG crosslinker gels that permit extensive remodeling but presented only the non-adhesive scrambled RDG sites from the ELPs exhibited minimal cell spreading due to the lack of suitable adhesive cues (Figure 3D). Similar to the 8-arm PEG crosslinked gels that could not be easily remodeled, the cells in the bis-functionalized PEG crosslinked gels presenting only non-adhesive RDG sites retained a rounded morphology (Figure 3E). Thus, cells require both the remodelability afforded by low network connectivity and a sufficient concentration of adhesive ligands to spread in 3D microenvironments.
2.4. Isonitrile-ChO crosslinked ELP-PEG hydrogels support the culture of various cell types
For the isonitrile-ChO ligation to be useful as a crosslinking reaction to prepare cell-encapsulating hydrogels for tissue engineering, the reaction must not detrimentally impact the human cell types required for a given application. To evaluate the biocompatibility of isonitrile-ChO crosslinking, multiple human cell types were encapsulated and cultured in isonitrile-ChO crosslinked ELP-PEG hydrogels. To enable cell spreading, all conditions used RGD-containing ELP-isonitrile crosslinked by PEG-bis-ChO. Human MRC5 fibroblasts were encapsulated in hydrogels with storage moduli of ~ 2 kPa, as this stiffness was shown above to enable robust cell spreading. Human vascular endothelial cells (HUVECs), human neural stem cells (hNSCs; ReNcell CX), and primary human myoblasts were encapsulated in hydrogels with storage moduli of ~400 Pa, consistent with prior reports.[2b, 17] Cell viability was assessed via live/dead staining to evaluate both acute (1 h) and longer term (2 d) cell health following the crosslinking reaction (Figure 4A,B). Consistent with the bioorthogonal nature of the isonitrile-ChO ligation, all cell types exhibited greater than 97% acute viability 1 h post-crosslinking. After two days in culture, cell viability remained similarly high, with fibroblasts approaching 90% viability and HUVECs, hNSCs, and myoblasts maintaining greater than 97% viability. Thus, the isonitrile-ChO crosslinking reaction is highly biocompatible with multiple human cell types.
Figure 4.

Isonitrile-ChO hydrogels maintain cell viability and proper function. (A) Representative live/dead fluorescence micrographs and (B) live/dead quantification demonstrating high cell viability for human fibroblasts, HUVECs, hNSCs, and human myoblasts maintained in isonitrile-ChO ELP-PEG hydrogels for 1 h or 2 d. (C) HUVECs in isonitrile-ChO ELP-PEG hydrogels stain positive for the endothelial marker CD31(green) and self-organize into tubular networks after 7 d in culture. Inset: Orthogonal view showing open lumen-like structure in region denoted by dashed white line. (D) Human NSCs encapsulated in isonitrile-ChO ELP-PEG hydrogels stain positive for the NSC stemness markers nestin (green) and Sox2 (red) after 7 d in culture and maintain their differentiation capacity, staining positive for the neuronal marker MAP2 and the astrocytic marker GFAP after an additional 7 d of differentiation. (E) Primary human myoblasts encapsulated in isonitrile-ChO ELP-PEG hydrogels stain positive for the myogenic progenitor markers Pax7 (red) and MyoD (yellow) and remain negative for the committed marker myogenin (MyoG; green) after 7 d in culture. The cultured myoblasts further maintain the capacity to differentiate into striated myotubes upon an additional 9 days of culture under differentiation conditions, staining positive for the mature myotube markers sarcomeric ⍺-actinin (SAA, red) and dystrophin (Dmd, yellow). The white arrow highlights the presence of striated sarcomeres. In B, data are presented as mean ± s.d., n = 3.
Beyond maintaining cell viability, hydrogel materials used as engineered ECM must support the proper function of pro-regenerative cell types to assemble functional tissue. For proper integration into host tissues, engineered tissues must be vascularized, and one strategy is to incorporate endothelial cells to preassemble blood vessels.[19] Thus, in our gels, encapsulated endothelial cells should not only survive crosslinking but also retain the ability to form 3D tubular networks. HUVECs were encapsulated in the isonitrile-ChO ELP-PEG hydrogels and cultured for 7 d prior to being fixed and immunostained. By 7 d, the cells had self-organized into networks of tubular structures and maintained expression of the endothelial marker CD31 (Figure 4C; Figure S18A, Supporting Information). Other common cell types used in tissue engineering are stem or progenitor cells that can differentiate into the mature cell types required for tissue-specific function. Neural stem cells are promising therapeutic targets to repair or replace damaged nervous tissue.[20] When cultured in the isonitrile-ChO ELP-PEG hydrogels for 7 d, hNSCs maintained expression of the neural stemness markers nestin and Sox2. Furthermore, culture for an additional 7 d in differentiation medium resulted in robust differentiation into neurons and astrocytes (Figure 4D; Figure S18B,C, Supporting Information), indicating that the encapsulated stem cells were indeed functional and capable of differentiating into the mature cell types of the central nervous system. Myoblasts are actively proliferating muscle progenitor cells that can subsequently differentiate and fuse into muscle fibers, suggesting that these cells could be used to generate engineered tissues to replace lost muscle tissue.[21] Primary human myoblasts cultured in the isonitrile-ChO ELP-PEG hydrogels for 7 d maintained expression of the progenitor markers Pax7 and MyoD, while remaining negative for the commitment marker myogenin (MyoG). Furthermore, the cultured cells could be subjected to differentiation conditions and yield striated myotubes that stained positive for the mature myotube markers sarcomeric α-actinin (SAA) and dystrophin (Dmd) (Figure 4E; Figure S19, Supporting Information). Taken together, these results indicate that isonitrile-ChO crosslinked ELP-PEG hydrogels support high viability and phenotypic maintenance of multiple human cell types relevant to tissue engineering.
2.5. Mutually orthogonal chemical functionalization of cellular microenvironments
An important advantage of bioorthogonal reactions is their ability to selectively chemically modify the hydrogel materials in the presence of live cells without having off-target effects on the cells. This could allow for conjugation of bioactive factors such as morphogens or adhesive ligands to direct cell differentiation and tissue organization. We first sought to demonstrate that the isonitrile ligation indeed enables bioorthogonal hydrogel functionalization by comparison to a non-bioorthogonal click reaction, thiol-maleimide addition. Thiol-functionalized RGD-ELP, in which 10 thiol groups were introduced at the primary amine sites in the ELP (RGD-ELP-10SH) and maleimide-functionalized bis-PEG crosslinkers (PEG-bis-maleimide) were synthesized. To form isonitrile ligation-based hydrogels, ten isonitrile groups per RGD-ELP-NC (5%, w/v) were reacted with PEG-bis-ChO (4.93%, w/v) to yield hydrogels with four excess isonitrile groups per ELP polymer, which could be labeled with fluorescent CF488A-Tz dye via isonitrile ligation. To form thiol-maleimide-based hydrogels, eight thiol groups per RGD-ELP-10SH (6.3%, w/v) were reacted with PEG-bis-maleimide (4.93%, w/v) to yield hydrogels with two excess thiols per ELP polymer, which could be labeled with fluorescent CF488A-Maleimide dye via maleimide-thiol addition. MRC5 fibroblasts were encapsulated in both types of gels and either immediately treated with fluorescent dyes in PBS or cultured for 7 days before being treated with dyes in complete cell culture medium (DMEM + 10% FBS). At both timepoints, non-reactive control dyes were included to demonstrate the specificity of the ligation reactions. The isonitrile ligation-based labeling exhibited the expected biorthogonality both initially and after 7 days of culture. Only treatment with tetrazine-containing dyes resulted in labeling of the hydrogels (Figure S20, Supporting Information). Moreover, voids were observed in the tetrazine-labeled hydrogels that corresponded to the location of the encapsulated cells, indicating that the isonitrile ligation reaction did not cross-react with biological functional groups present on the cells. Validating our spectroscopic analysis of isonitrile stability (Figure S8, Supporting Information), the gels were still able to be stained with tetrazine dyes after a week in culture, indicating that isonitrile groups are still present.
In contrast, the experiments with the maleimide-thiol crosslinked gels exhibited markedly less bioselectivity. Upon initial treatment with the fluorescent dyes in PBS, the excess thiols in the gels were stained only by the maleimide dye, but not by the control dyes. However, the cells encapsulated within the gels were also labeled by the maleimide dye, indicating that the maleimide-thiol addition cross-reacts with free thiols present on the surface of living cells (Figure S21A, Supporting Information). By day 7 of culture, substantial degradation of the gels was observed, as indicated by extensive cell spreading and sedimentation (Figure S21B, Supporting Information). Maleimide-thiol linkages are susceptible to retro-Michael addition reactions and thiol exchange with free thiols in the medium,[22] resulting in degradation of the gels and demonstrating markedly less stability in complex biological mixtures than the isonitrile ligation-based gels. When treated with maleimide-functionalized dye in complete cell culture medium, minimal labeling was observed in the maleimide-thiol gels, due in part to gel degradation and in part to cross-reactivity with thiols in the medium. Some labeling of cellular proteins was still observed. Taken together, these results demonstrate the bioorthogonality of the isonitrile ligation reaction, which contrasts with the limited selectivity of maleimide-thiol crosslinking strategies.
We have previously demonstrated the ability to functionalize materials in the presence of live cells using excess azides in hydrogels via SPAAC reactions.[23] We hypothesized that the addition of isonitrile ligation reactions would permit dual, mutually orthogonal functionalization of the hydrogels to sequentially conjugate two different factors. To demonstrate the mutual orthogonality of isonitrile-ChO ligation and SPAAC reactions, isonitrile and azide bifunctional RGD-ELP was synthesized by sequential reaction of the ELP primary amines with azidoacetic acid NHS ester and perfluorophenyl 3-isocyanopropanoate. The stoichiometric ratios of reactants were tuned to afford approximately 2 azides and 12 isonitriles per ELP polymer. To form hydrogels, ten isonitrile groups per polymer were reacted with PEG-bis-ChO to form hydrogels with two excess isonitriles and two free azides per ELP polymer, which could subsequently be labeled with fluorescent dyes via isonitrile ligation and SPAAC, respectively (Figure 5A). Control gels that consisted of purely isonitrile or purely azide functionalized ELPs crosslinked with PEG-bis-ChO or azide-reactive PEG-bis-DBCO, respectively, were also prepared. The gels were analyzed by oscillatory rheology and exhibited similar storage moduli (Figure 5B), while the SPAAC-crosslinked gels exhibited more rapid gelation kinetics (Figure 5C). Fibroblasts were encapsulated in the hydrogels and cultured for 7 days.
Figure 5.

Isonitrile ligation and SPAAC enable mutually orthogonal chemical functionalization of cell encapsulating hydrogels. (A) Schematic illustration of dual isonitrile and azide functionalized RGD-ELP crosslinked with PEG-bis-ChO and subsequently modified with CF488A-Tz and CF640R-BCN fluorescent dyes. (B) Storage moduli and (C) gelation times for dual isonitrile and azide functionalized or pure isonitrile and pure azide functionalized ELP-PEG hydrogels. (D) Representative fluorescence micrographs of cell-encapsulating hydrogels after treatment with fluorescent dyes. The actin cytoskeleton was stained with phalloidin (orange), the nuclei were stained with DAPI (blue), and hydrogels were reacted with CF488A (green) and CF640R (magenta) dyes. Quantification of relative fluorescence intensity from digested ELP-PEG hydrogels after treatment with CF488A and CF640R dyes at excitation wavelengths of (E) 460 and (F) 600 nm. In B, C, E, and F, data are presented as mean ± s.d., n = 3. In E and F, ****p<0.0001 relative to amine dye controls, one-way ANOVA with Bonferroni post-hoc test.
To demonstrate orthogonal functionalization via isonitrile ligation and SPAAC, the hydrogels containing live cells were sequentially treated with the green-fluorescent tetrazine-containing dye CF488A-Tz and the far-red-fluorescent cyclooctyne-containing dye CF640R-BCN in complete cell culture medium. As negative controls, separate subsets of hydrogels were left untreated or were treated with the non-reactive amine-containing versions of the CF488A and CF640R dyes. After washing out unreacted dye, the gels were fixed, and the cells were stained with DAPI and phalloidin prior to imaging. As expected, the untreated and amine-dye treated negative controls exhibited negligible fluorescence from either dye (Figure 5D). The isonitrile and azide dual-functionalized ELP hydrogels showed strong fluorescent signals for both dyes, indicating that both the Tz and BCN dyes could chemically conjugate to the hydrogel network. Importantly, the control gels containing only excess isonitriles only reacted with the CF488A-Tz, and the control gels containing only excess azides only reacted with the CF640R-BCN. Thus, the isonitrile-Tz and azide-BCN reactions are mutually orthogonal when performed sequentially and enable dual bioorthogonal functionalization of cell-encapsulating hydrogels. To validate the microscopy results, a second set of hydrogels were exposed to the same conditions before being digested with trypsin to quantify the fluorescent dye incorporation with a fluorescence microplate reader. Consistent with the microscopy results, significant dye incorporation over background was observed only when excess isonitriles were present for the CF488A-Tz and only when excess azides were present for the CF640R-BCN (Figure 5E,F; Table S1,2, Supporting Information).
3. Discussion
The reactions used to form cell-encapsulating hydrogels must proceed rapidly and efficiently to reproducibly form gel networks fast enough to ensure homogeneous cell distributions. Accordingly, a class of chemistries often referred to as “click” reactions are frequently employed.[24] To avoid perturbing cellular biochemistry during crosslinking, the reactions should also be bioorthogonal.[23, 25] Many “click” chemistries do not meet this higher threshold, as they make use of functional groups that cross-react with biological chemistries (e.g., maleimide-thiol conjugation) or metal catalysts that could be toxic to cells (e.g., copper-catalyzed azide-alkyne cycloaddition). Nevertheless, these chemistries are routinely employed to produce cell encapsulating hydrogels, as the decrease in chemical selectivity is weighed against lower cost, commercial availability, and/or synthetic simplicity. Two bioorthogonal reactions exhibit sufficiently rapid kinetics for gelation: SPAAC and tetrazine-mediated IEDDA.[23] Of the two, SPAAC is ideal, as azides are small and very stable in physiological conditions. Both tetrazines and their corresponding dienophiles are relatively large and often hydrophobic, which can detrimentally impact the solubility of hydrogel components, and tetrazines are prone to degradation in aqueous environments.[26] Based on our results, we propose that isonitrile ligations can serve a similar role compared to SPAAC as an ideal bioorthogonal crosslinking reaction to engineer cell-encapsulating hydrogels. Like azides, isonitriles are small and soluble, and we demonstrate that isonitriles do not impair the solubility of ELPs, which are quite sensitive to conjugation of hydrophobic chemical moieties. Further, isonitriles are also stable under physiological conditions, as demonstrated by their ability to react with tetrazine-bearing fluorescent dyes even after 7 days of cell culture (Figure 5D–F). Our results position isonitriles among the least disruptive chemical mechanisms for dynamically altering cell encapsulating hydrogels, along with SPAAC[2b] and emerging technologies leveraging visible or near-infrared light triggered reactions[27] and biochemical approaches using non-mammalian enzymes.[28]
Another major advantage of hydrogel networks formed by step-growth, click-type bioorthogonal reactions is the precise control afforded over the network architecture. As long as the locations of the reactive groups on the polymer chain can be controlled, the resulting networks will have well-defined crosslink spacing, which will result in consistent mesh size, homogenous mechanical properties, and control over network degradation. The localization of reactive groups to the ends of the PEG arms and to the primary amines within the engineered ELP sequence enables this control in the ELP-PEG hybrid systems. Due to the selectivity of the isonitrile-ChO ligation, the crosslinks are restricted to the elastin-like domains of the proteins, whereas degradation by cell secreted proteases typically occurs in the bioactive domains.[17, 20b] Thus, by varying the functionality of the PEG crosslinkers, the extent of degradation of the networks can be tuned,[17] providing control over the extent of cell spreading in the hydrogels (Figure 3), while independently controlling stiffness and adhesive ligand presentation, which also regulate cell spreading.[2b]
The bioorthogonality of isonitrile ligations makes these chemistries attractive for in vivo applications, such as the injection of hydrogel-based carriers for cells and therapeutic agents. The crosslinking kinetics of the isonitrile-ChO ligation in particular provide sufficient time to mix the hydrogel precursors with therapeutic agents and then inject the pre-gel solution into the target tissue prior to gelation. As other bioorthogonal reactions such as the Staudinger ligation and SPAAC have been demonstrated to selectively react in live animals,[29] we anticipate that isonitrile ligations will enable hydrogel formation without off-target effects on host tissues. Future work is necessary to optimize the hydrogel formulations prepared in this study for injectable delivery of therapeutically relevant cell types into preclinical animal models.
The identification of a bioorthogonal reaction that is also mutually orthogonal to SPAAC opens up new possibilities for multi-stage modification of cellular microenvironments. In the present work, we demonstrate that hydrogels presenting both azides and isonitriles can be selectively functionalized with fluorescent dyes bearing cyclooctyne and tetrazine moieties, respectively. This result suggests that tissue engineering scaffolds can be sequentially functionalized with two different biochemical factors to temporally control tissue development. Such mutually orthogonal functionalization could also enable localized sequential delivery of therapeutic agents to hydrogel scaffolds in vivo. Suggesting such an approach may be feasible, SPAAC has previously been used to localize chemotherapeutic agents to azide-bearing hydrogels at tumor sites in a mouse model.[30] Beyond altering biochemical factors, incorporation of two distinct bioorthogonal chemistries may also enable in situ tuning of hydrogel mechanical properties, for instance, by using the isonitriles to add secondary crosslinks and stiffen the network. Thus, we anticipate hydrogel scaffolds utilizing isonitrile ligations to find broad use in tissue engineering and drug delivery applications.
4. Conclusion
Isonitriles react with chlorooximes, azomethine imines, and tetrazines to yield stably crosslinked hydrogels. Isonitrile-chlorooxime crosslinking exhibited the most rapid gelation kinetics, while proceeding at physiological pH and without generation of gaseous byproducts, making it best suited for preparing cell-encapsulating hydrogels. The resulting gels exhibited tunable, predominantly elastic mechanical properties. The selectivity of the isonitrile-chlorooxime ligation enabled independent tuning of network connectivity and cell adhesive ligand density in ELP-PEG hydrogels, which in turn regulated the spreading of encapsulated cells. The bioorthogonal nature of the isonitrile-chlorooxime ligation permitted encapsulation of multiple human cell types, which maintained high viability and proper phenotype for up to two weeks in culture. Furthermore, the stability of the isonitriles and orthogonality of isonitrile ligation and SPAAC provided the ability to sequentially and selectively functionalize cell-encapsulating hydrogels with model small molecules. These results indicate that isonitrile ligations are useful bioorthogonal reactions for engineering cellular microenvironments, especially as participants in multicomponent reactions to develop complex hydrogel materials as ECM-mimicking scaffolds for tissue engineering.
5. Experimental Section
General:
Reagents used for the synthesis of hydrogel precursors were purchased from Fisher Scientific, Sigma-Aldrich, Honeywell, or BLDpharm, unless otherwise noted. Water-sensitive reactions were conducted using commercially available anhydrous solvents. PEG precursors were purchased from JenKem Technology. Cell culture reagents were purchased from Thermo Fisher Scientific or Lonza. Rheological characterization was performed using a Rheometrics ARES-RFS3 strain controlled rheometer. Fluorescence microscopy images were collected on Zeiss LSM 900 laser scanning confocal microscope equipped with a broadband (385–730 nm) widefield epifluorescence light source and a Photometrics Prime BSI camera. FT-IR data were collected on a JASCO FT/IR-6300 Spectrometer. Fluorescence intensity measurements were performed using a Tecan Infinite® M Plex multimode microplate reader. 1H and 13C NMR spectra were recorded on a Bruker NEO 400 or 600 spectrometer at 400 MHz or 600 MHz, respectively. Chemical shifts are reported in parts per million (ppm) and are referenced to the residual solvent peak (CDCl3, δ1H = 7.26 ppm, δ13C = 77.16 ppm, and DMSO-d6, δ1H = 2.50 ppm, δ13C = 39.52 ppm). The following abbreviations were used s (singlet), d (doublet), t (triplet) and m (multiplet). Human fetal lung fibroblasts (MRC5) were purchased from the American Type Culture Collection (ATCC, CCL-171). Human umbilical vein endothelial cells (HUVECs) were purchased from Lonza (C2519A). Human NSCs (ReNcell CX, SCC007) were purchased from Millipore Sigma. Primary human myoblasts were a kind gift from Prof. Helen Blau (Stanford University).
Synthesis and Characterization of Pentafluorophenyl 3-isocyanopropanoate:
The amine-reactive isonitrile precursor was synthesized by modifying published procedures.[11] 3-aminopropanoic acid (3.5 g, 33.4 mmol, 1.0 eq.) was dissolved in formic acid (34 mL), and acetic anhydride (12.6 g, 123.2 mmol, 3.7 eq.) was added. The reaction was stirred at 50°C for 2 h. The mixture was diluted with water (100 mL) and concentrated. The obtained 3-formamidopropanoic acid (3 g) was used without further purification. 3-formamidopropanoic acid (2.34 g, 20 mmol, 1.0 eq.) was suspended in anhydrous THF (120 mL). Pentafluorophenol (4.04 g, 22 mmol, 1.1 eq.) and N,N’-dicyclohexylcarbodiimide (4.54 g, 22 mmol, 1.1 eq.) were added, and the reaction mixture was stirred at r.t. for 3 h. The precipitate was filtered and washed with DCM. The combined filtrates were concentrated to afford the product as a colorless oil in 83% yield (4.7 g), which was used immediately without further purification. N-formyl-β-alanine 2,3,4,5,6-pentafluorophenyl ester (4.7 g, 16.6 mmol, 1 eq.) was dissolved in anhydrous THF (200 mL). The solution was cooled to 0°C and triethylamine (41.5 mmol, 2.5 eq.) was added, followed by POCl3 (20.8 mmol, 1.25 eq.). The reaction was stirred until the starting material was consumed as visualized by thin-layer chromatography (TLC 1:4, EtOAc:Hexane). The reaction mixture was diluted with DCM (100 mL) and quenched by addition of aqueous 2M NaHCO3. The phases were separated in a separatory funnel, and the organic phase was washed by agitating with aqueous 2M NaHCO3 (2x) and then with brine. The organic phases were dried by adding anhydrous MgSO4, filtered, and concentrated by rotary evaporation until a solid was obtained. The crude yellow crystalline product was further purified by column chromatography (1:4 EtOAc:Hexane). The pure product was obtained as a white crystalline solid in 75% yield. The 1H NMR and 13C NMR spectra are provided in the ESI (Figure S22–23, Supporting Information). 1H NMR (400 MHz, CDCl3, δ): 3.83 (t, J = 6.8 Hz, 2H), 3.13 (t, J = 6.8 Hz, 2H). 13C NMR (151 MHz, CDCl3, δ) 165.77, 159.14, 142.01, 141.98, 141.95, 141.92, 141.89, 140.92, 140.83, 140.36, 140.33, 140.31, 140.28, 140.25, 140.22, 140.19, 139.15, 139.01, 138.91, 138.89, 138.87, 138.81, 137.33, 137.26, 137.22, 137.14, 137.11, 124.62, 36.92, 36.87, 36.83, 33.55.
Synthesis and Characterization of 8-arm PEG-NC:
8-arm PEG-amine (1000 mg, MW ~ 20 kDa, 0.40 mmol −NH2, 1 eq.) and pentafluorophenyl 3-isocyanopropanoate (138 mg, 0.52 mmol, 1.3 eq.) were added to a round bottom flask containing a stir bar and dissolved in anhydrous DMF (8 mL). After complete dissolution of the reagents, triethylamine (335 μL, 2.4 mmol, 6.0 eq.) was added, and the mixture was stirred at room temperature overnight. The PEG was precipitated by dropwise addition to ice cold diethyl ether (3 × 45 mL) and collected by centrifugation. The supernatant was decanted, and the pellet was washed with cold ether (45 mL), dried under a stream of compressed air, and re-dissolved in water (15 mL). The solution was dialyzed against water (MWCO 2 kDa, 4× 4.5 L, 4°C), flash frozen in liquid nitrogen, and lyophilized to afford the light-yellow product in 90% yield.
Synthesis and Characterization of PEG-benzylaldehyde:
PEG-bis-amine (500 mg, 0.133 mmol, 1 eq., 7.5 kDa) and N-succinimidyl 4-formylbenzoate[31] (49.4 mg, 0.2 mmol, 1.5 eq.) were added to a two-neck round bottom flask and dissolved in N,N-dimethylformamide (8 mL). N,N-diisopropylethylamine (139 μL, 6 eq.) was added to the mixture, and the reaction was allowed to proceed at room temperature overnight. The PEG was precipitated in cold diethyl ether and collected by centrifugation. The crude product was washed with cold diethyl ether, centrifuged, and dried to obtain PEG-bis-benzylaldehyde as a white solid in 92% yield. 3-arm PEG-benzaldehyde (15 kDa) and 8-arm PEG-benzaldehyde (20 kDa and 40 kDa) were prepared from 3-arm and 8-arm PEG-amine precursors following the same procedure in 93%, 96%, and 92% yield, respectively. 1H NMR characterization is provided in the ESI (Figure S24–27, Supporting Information).
Synthesis and Characterization of PEG-benzaldehyde oxime:
PEG-bis-benzylaldehyde (500 mg, 0.133 mmol, 1 eq.) and hydroxylamine hydrochloride (185 mg, 2.66 mmol, 20 eq.) were added to a two-neck round bottom flask. Methanol (8 mL) was added to flask, and the reaction mixture was stirred at room temperature for 2 days. The mixture was concentrated in vacuo, redissolved in DCM, washed with HCl (1 M, 2 × 15 mL) and water (15 mL), dried with Mg2SO4, concentrated to few milliliters, and precipitated in cold diethyl ether. The crude product was washed with cold diethyl ether and dried under vacuum to provide the product as a white solid in 91% yield. 3-arm PEG-benzaldehyde oxime (15 kDa) and 8-arm PEG-benzaldehyde oxime (20 kDa and 40 kDa) were prepared from 3-arm and 8-arm PEG-benzaldehyde precursors following the same procedure in 88%, 81%, and 76% yield, respectively. 1H NMR characterization is provided in the ESI (Figure S28–31, Supporting Information).
Synthesis and Characterization of PEG-ChO:
PEG-chlorooximes were synthesized based on previously published procedures.[12a] PEG-bis-benzaldehyde oxime (440 mg, 0.12 mmol, 1 eq.) and N-chlorosuccinimide (23.5 mg, 0.18 mmol, 1.5 eq.) were added to a two-neck round bottom flask and dissolved in N,N-dimethylformamide (4 mL). The reaction mixture was stirred at room temperature overnight. The PEG was precipitated by dropwise addition to cold diethyl ether. The crude product was washed with cold diethyl ether, redissolved in methanol (2.5 mL), dialyzed against methanol for 24 h (3 × 350 mL, r.t.), precipitated in cold diethyl ether, and dried under vaccum to provide the product as a white powder in 91% yield. 3-arm PEG-chlorooxime (15 kDa) and 8-arm PEG-chlorooxime (20 kDa and 40 kDa) were prepared from 3-arm and 8-arm PEG-benzaldehyde oxime precursors following the same procedure in 84%, 85%, and 88% yield, respectively. 1H NMR characterization is provided in the ESI (Figure S32–35, Supporting Information).
Synthesis and Characterization of AMI:
An amine-bearing azomethine imine precursor was prepared based on reported procedures.[9] Methyl 4-(((tert-butoxycarbonyl)amino)methyl)benzoate (250 mg, 0.94 mmol, 1 eq.) was suspended in MeOH (3 mL). Hydrazine monohydrate (0.301 mL, 9.4 mmol, 10 eq.) was added, and the mixture was stirred at 90 °C overnight. The mixture was dried in vacuo, and then water was added dropwise to produce a suspension. tert-butyl (4-(hydrazinecarbonyl)benzyl)carbamate was obtained by filtration as a white solid in 90% yield. The 1H NMR characterization is provided in the ESI (Figure S36, Supporting Information). 1H NMR (400 MHz, DMSO-d6, δ): 9.69 (s, 1H), 7.76 (d, J = 8.1 Hz, 2H), 7.42 (t, J = 6.2 Hz, 1H), 7.28 (d, J = 8.0 Hz, 2H), 4.45 (d, J = 3.8 Hz, 2H), 4.15 (d, J = 6.2 Hz, 2H), 1.39 (s, 9H). tert-butyl (4-(hydrazinecarbonyl)benzyl)carbamate (250 mg, 0.95 mmol, 1 eq.) was added to a round bottom flask with 2-(2-bromoethyl)benzaldehyde (201 mg, 0.95 mmol, 1 eq.). Methanol (4 mL) was added, and the mixture was stirred at 80 °C for 3 h. After cooling to room temperature, the mixture was treated with triethylamine (143 mg, 2.8 mmol, 1.5 eq.), poured into water, and stirred for 15 minutes. The suspension was filtered, washed with cold water, dried under vacuum, dissolved in DCM, dried over MgSO4, and concentrated in vacuo. (4-(((tert-butoxycarbonyl)amino)methyl)benzoyl)(3,4-dihydroisoquinolin-2-ium-2-yl)amide was obtained as a yellow solid (70%) and used without further purification. (4-(((tert-butoxycarbonyl)amino)methyl)benzoyl)(3,4-dihydroisoquinolin-2-ium-2-yl)amide (545 mg, 1.44 mmol) and 4 M HCl in dioxane solution (4 mL) was added to a round bottom flask. The mixture was stirred at room temperature for 2 h. The mixture was concentrated in vacuo to yield mono(2-(4-(ammoniomethyl)benzamido)-3,4-dihydroisoquinolin-2-ium) dichloride as a light-yellow solid in 90% yield. The 1H NMR characterization is provided in the ESI (Figure S37, Supporting Information). 1H NMR (400 MHz, DMSO-d6, δ): 9.69 (s, 1H), 8.62 (s, 3H), 8.13 (d, J = 8.1 Hz, 2H), 7.95 (d, J = 7.6 Hz, 1H), 7.87 (t, J = 7.6 Hz, 1H), 7.69 (d, J = 8.0 Hz, 2H), 7.65 – 7.50 (m, 2H), 4.43 (t, J = 8.0 Hz, 2H), 4.13 (q, J = 5.9 Hz, 2H), 3.40 (t, J = 8.1 Hz, 2H).
Synthesis and Characterization of 8-arm PEG-AMI:
8-arm PEG-NHS (100 mg, 0.04 mmol NH2, 1 eq., 20 kDa) and the azomethine imine precursor prepared above (18.3 mg, 0.052 mmol, 1.3 eq.) were added to a two-neck round bottom flask. Anhydrous N,N-dimethylformamide (3 mL) was added with stirring. N,N-diisopropylethylamine (42 μL, 6 eq.) was added to the mixture, and the reaction was allowed to proceed at room temperature overnight. The mixture was directly dialyzed against cold MilliQ water for 2 days (4 × 4.5L, 4 °C), flash frozen in liquid nitrogen, and lyophilized to obtain a white powder in 91% yield. 1H NMR characterization is provided in the ESI (Figure S38, Supporting Information).
Synthesis and Characterization of 8-arm PEG-Tz:
8-arm PEG-amine (100 mg, 0.04 mmol NH2, 1 eq., 20 kDa) and methyltetrazine-NHS ester (Click Chemistry Tools, 17 mg, 0.052 mmol, 1.3 eq.) were added to a two-neck round bottom flask. Anhydrous N,N-dimethylformamide (2.5 mL) was added with stirring. N,N-diisopropylethylamine (42 μL, 6 eq.) was added, and the reaction was allowed to proceed at room temperature overnight. The mixture was directly dialyzed against cold MilliQ water for 2 days (4 × 4.5L, 4 °C), flash frozen in liquid nitrogen, and lyophilized to obtain a magenta powder in a quantitative yield. 1H NMR characterization is provided in the ESI (Figure S39, Supporting Information).
Synthesis and Characterization of 7.5 kDa PEG-bis-Maleimide:
PEG-bis-amine (200 mg, MW ~ 7.5 kDa, 0.053 mmol −NH2) and succinimidyl-4-(N-maleimidylmethyl)cyclohexane-1-carboxylate (26.8 mg, 1.5 eq relative to amines, 0.08 mmol) were added to a 25 mL round bottom flask and dissolved in anhydrous DMF (4 mL). N,N- diisopropylethylamine (27.9 μL, 3 eq, 0.16 mmol) was added, and the reaction was allowed to proceed overnight at room temperature. The maleimide-modified PEG was precipitated by dropwise addition to ice cold diethyl ether (40 mL) and collected by centrifugation. The pellet was washed with ice cold diethyl ether (2×40 mL) and dried under a stream of compressed air. The resulting white solid was redissolved in MilliQ water (10 mL) and dialyzed against MilliQ water (MWCO 2 kDa, 4°C, 4×4.25 L). The resulting solution was frozen with liquid nitrogen and lyophilized to afford the PEG-bis-maleimide as a white solid (180 mg, 90% yield). 1H NMR characterization is provided in the ESI (Figure S41, Supporting Information).
Expression and Characterization of ELPs:
The ELPs used in this study were originally developed by Straley and Heilshorn.[18] Plasmids encoding these proteins were a kind gift from Prof. Sarah Heilshorn (Stanford University). To improve the yield of recombinantly expressed ELPs, both the RGD (cell adhesive) and RDG (non-cell adhesive) ELP genes were cloned into an improved pET15b construct with a corrected T7 promoter site (pET15b-T7pCONS sfGFP), obtained via Addgene (#154467) courtesy of Prof. Daniel Daley (University of Stockholm) via restriction-ligation cloning using NcoI and BamHI (RGD) or NcoI and BlpI (RDG) restriction enzymes and Instant Sticky End Ligase Mix (New England Biolabs).[32] Plasmids containing RGD-ELP and RDG-ELP were transformed into BL21(DE3)pLysS Escherichia coli (Thermo Fisher Scientific, C606003) and expressed under control of the T7 promoter. Bacteria were cultured in Terrific Broth at 37 °C to an OD600 of 0.8, and the addition of 1 mM isopropyl β-D-1-thiogalactopyranoside (IPTG) induced protein expression. The culture temperature was reduced to 32 °C, and the protein was allowed to express for 7 hours before the bacteria were harvested by centrifugation. Bacterial pellets were resuspended in TEN buffer (10mM Tris, 1mM EDTA, and 100mM NaCl, pH 8.0) and lysed using repetitive freeze-thaw cycles. DNAse1 and 1mM phenylmethylsulphonyl fluoride (PMSF) were added to lysates to remove genomic DNA and to inhibit proteases, respectively. The thawed lysates were adjusted to pH 9.0 using NaOH and purified through inverse temperature cycling.[33] The resulting ELP solution was desalted by dialyzing against MilliQ water (4 × 4.5 L, 4 °C). The dialyzed ELP solutions were frozen at −80 C and lyophilized for 3 days to obtain a white solid. Expression of ELP-RGD and ELP-RDG yielded 2.08 g and 1.37 g, respectively, from 12 L of bacterial culture. Protein identity was confirmed post-expression by SDS-PAGE (Figure S10, Supporting Information).
Synthesis and Characterization of Isonitrile- and Azide-Functionalized ELPs:
To functionalize ELPs with isonitriles, ELP (100 mg, 0.037 mmol -NH2, 38 kDa) was dissolved in anhydrous dimethyl sulfoxide (DMSO, 5 mL) to a final concentration of 2% (w/v). Perfluorophenyl 3-isocyanopropanoate (12.8 mg, 0.048 mmol, 1.3 eq.) was added to the ELP solution, followed by addition of triethylamine (10 μL, 0.072 mmol, 1.5 eq to isonitrile group) as a basic catalyst. The reaction mixture was stirred at room temperature overnight. The isonitrile-functionalized ELP was dialyzed against cold water (4 × 4.5 L, 4 °C) and lyophilized to afford RGD-ELP-NC (90% yield) and RDG-ELP-NC (90% yield) as light-yellow solids. The same procedure was used to prepare azide-functionalized ELPs, replacing the perfluorophenyl 3-isocyanopropanoate with azidoacetic acid NHS ester (9.5 mg, 0.048 mmol, 1.3 eq.) and producing a light-yellow solid in 90% yield. To prepare isonitrile and azide dual-functionalized ELP, RGD-ELP was dissolved in anhydrous dimethyl sulfoxide (DMSO) to a final concentration of 2% (w/v). 2/14 equivalents of azidoacetic acid NHS ester were added to the RGD-ELP solution while stirring. Triethylamine (1.5 eq to NC) was then added as a basic catalyst. The reaction was allowed to proceed for 24 h at room temperature with stirring. Then, excess perfluorophenyl 3-isocyanopropanoate (14.6 mg, 1.5 eq. to NH2) was added to the N3-functionalized ELP mixture, the reaction was continued overnight. The RGD-ELP-N3/NC was purified by dialyzing against cold water (4 × 4.5 L, 4 °C) and lyophilized to afford the product as a light-yellow solid in quantitative yield. The ELPs were considered to be fully modified with isonitriles and/or azides based on 1H NMR spectra showing a disappearance of the lysine peak at 2.72 ppm. The 1H NMR spectra are included in the ESI (Figure S11 and Figure S42–44, Supporting Information).
Synthesis and Characterization of RGD-ELP-7/10/14SATA:
To functionalize ELPs with thiols, ELP (100 mg, 0.037 mmol -NH2, 38 kDa) was dissolved in anhydrous dimethyl sulfoxide (DMSO, 5 mL) to a final concentration of 2% (w/v). N-succinimidyl-S-acetylthioacetate (SATA, 4.3 mg, 0.018 mmol, to react with 7-NH2, 0.5 eq.; 6.1 mg, 0.026 mmol, to react with 10-NH2, 0.71 eq.; 11.1 mg, 0.048 mmol, to react with 14-NH2, 1.3 eq.) was added to the ELP solution, followed by addition of triethylamine (10 μL, 0.072 mmol, 1.5 eq to isonitrile group) as a basic catalyst. The reaction mixture was stirred at room temperature overnight. The SATA-functionalized ELP was dialyzed against cold water (4 × 4 L, 4 °C) and lyophilized to afford RGD-ELP-7/10/14SATA (85%, 88% and 90% yield, respectively) as white solids. In comparing the three products, the stacked 1H NMR spectra show a complete disappearance of the lysine peak at 2.72 ppm in RGD-ELP-14SATA, a small residual peak remaining in RGD-ELP-10SATA, and stronger peak remaining in RGD-ELP-7SATA (Figure S48, Supporting Information). The complete 1H NMR spectra are included in the ESI (Figure S45–47, Supporting Information).
Synthesis and Characterization of RGD-ELP-7/10/14SH:
A deprotection solution was prepared by dissolving 1.74 g hydroxylamine·HCl and EDTA (0.465 g of disodium salt) in 40 mL of PBS, adjusting the pH to 7.2–7.5 with NaOH, and bringing to a final volume of 50 mL. Separately, RGD-ELP-7/10/14SATA samples were dissolved in PBS at 4 °C with stirring overnight. The deprotection solution was added to the ELP solutions separately (~ 40 eq. of hydroxylamine to SATA). The reaction mixture was stirred at 4 °C for two days, dialyzed against cold water (4 × 4 L, 4 °C), and lyophilized to afford RGD-ELP-7/10/14SH (~ 90% yield) as white solids. 1H NMR spectra showed a disappearance of the methyl peak at 2.33 ppm, indicating complete deprotection and successful synthesis of thiol-functionalized ELPs. 1H NMR spectra are included in the ESI (Figure S49–51, Supporting Information).
Hydrogel formation:
PEG precursor solutions were prepared by dissolving the functionalized PEGs in PBS at room temperature for 20 min, and then maintaining the solutions on ice until used. For the experiments testing the pH-dependence of the isonitrile-AMI ligation, the pH of the PBS was adjusted to pH 6, 6.5, or 7 prior to dissolving the PEG. The ELP precursor solutions were prepared by dissolving the ELP-isonitrile in PBS at 4 °C overnight, and then maintaining the solutions on ice until used. The concentrations of the precursor solutions were chosen to maintain a 1:1 molar ratio of reactive groups. Hydrogels were prepared by mixing the two precursor solutions in either a 3:2 (v/v) ratio (isonitrile to ChO, AMI, and Tz) for pure PEG gels or a 1:1 (v/v) ratio for ELP-PEG hybrid gels.
Rheological Characterization:
Hydrogel precursor solution prepared as described above were gelled in situ on a Peltier stage and subjected to oscillatory rheology using a 25 mm 0.02 radian cone geometry. Gelation of purely PEG gels were performed at either 22 °C or 37 °C, while ELP-PEG gels were added to the Peltier stage at 4 °C and then raised to 22 °C to prevent protein phase separation prior to gelation. Time sweeps were performed at 5% strain and 1 Hz oscillatory frequency. The gelation time was determined as the point at which the storage modulus (G’) first exceeded the loss modulus (G”). Frequency sweeps were performed at 37 °C and a fixed strain of 5% with oscillatory frequencies spanning 0.1 to 10 Hz. Strain sweeps were performed at 37 °C and fixed 1 Hz oscillatory frequency from an initial strain of 0.1% to a final strain 10%.
Hydrogel Stability:
Solutions of 5% 8-arm PEG-NC, 5% 8-arm PEG-ChO, 5% 8-arm PEG-AMI and 5% 8-arm PEG-Tz were prepared in PBS at room temperature (w/v). For isonitrle-ChO hydrogels, 50 uL of hydrogels were cast in pre-weighed vials and kept at room temperature until crosslinking was completed. For isonitrle-AMI or Tz hydrogels, 50 uL of hydrogels were cast in pre-weighed vials and incubated at 37 °C until crosslinking was complete. One mL of either PBS or complete cell culture medium (DMEM + 10% FBS) was added to the vials, and the samples were kept at 37 °C. To evaluate hydrogel degradation, the supernatant was carefully removed to measure the wet mass of hydrogels. After measuring the wet mass, the samples were frozen and lyophilized. The dry mass of the hydrogels was then measured. Mass loss over time was determined from the hydrogel dry mass measurements. Hydrogel mass swelling ratios were calculated by dividing the wet mass by the dry mass of the samples.
Cell Culture and Encapsulation:
Fibroblasts were cultured and expanded in high glucose Dulbecco’s modified Eagle medium (DMEM) plus GlutaMAX, 10% fetal bovine serum (FBS) and 1% penicillin/streptomycin (P/S). HUVECs were cultured and expanded in EGM-2 medium (Lonza). Human NSCs were cultured and expanded in ReNcell™ NSC maintenance medium, 20 ng/mL fibroblast growth factor-2 (FGF-2), and 20 ng/mL epidermal growth factor (EGF) on polyornithine- and laminin-coated tissue culture dishes. Myoblasts were cultured and expanded in Ham’s F-10 Nutrient Mix, 20% FBS, 2.5 ng/mL FGF-2, and 1% penicillin/streptomycin on collagen-coated tissue culture dishes. Prior to encapsulation in hydrogels, cells were lifted with trypsin, collected by centrifugation, and counted using a hemocytometer. Cells were mixed with the pre-gel solutions to yield the following final cell densities: 1× 106 mL−1 for fibroblasts, 2 × 107 mL−1 for HUVECs, 5 × 107 mL−1 for NSCs, and 2 × 107 mL−1 for myoblasts. Fibroblasts were mixed with 3% RGD-ELP-NC+1.5% RDG-ELP-NC that were crosslinked with 6.2% PEG-bis-ChO (all w/v) to yield a storage modulus of 2185 Pa. HUVECs, hNSCs, and myoblasts were mixed with 3% RGD-ELP-isonitrile that was crosslinked with 4.14% PEG-bis-ChO, to yield hydrogels with a storage modulus of 385 Pa. The volume ratio for each component was held constant as 1:1 (v:v).
The gels were then cast in custom cylindrical silicone molds and cultured in either maintenance medium or differentiation medium. For hNSC differentiation, after 7 d in maintenance medium, the cells were cultured for an additional 7 d in the base maintenance medium without FGF-2 and EGF to induce differentiation. For myoblast differentiation, after 7 d in maintenance medium, the cells were cultured for 2 d in F-10 Nutrient Mix plus 20% FBS without grow factor, followed by 7 d in high glucose DMEM plus 2% horse serum, 1% penicillin / streptomycin and 10 μg mL−1 insulin.
Cell Viability:
After crosslinking was complete, cell-encapsulating hydrogels were submerged in maintenance medium and incubated at 37 °C and 5% CO2. For acute viability, cells were cultured for 1 h post-crosslinking. To assess longer term viability, cells were cultured for 2 d post-crosslinking. Live/dead staining was performed by incubating cells with calcein-AM (1 μM) and ethidium homodimer (1μM) in base DMEM for 45 min, washing with base DMEM and imaging via confocal microscopy.
Immunofluorescence Analysis:
To assess cell morphology, samples were fixed with 4% paraformaldehyde in PBS for 45 min at 37 °C, permeabilized with 0.25% Triton X-100 in PBS (PBST) for 30 min, stained with phalloidin-tetramethylrhodamine B isothiocyanate and DAPI in PBS for 40 min at room temperature, washed with PBST, and then imaged by confocal microscopy. Expression of protein factors indicating proper phenotypes for HUVECs, hNSCs, and myoblasts was assessed by immunocytochemistry. Samples were fixed with 4% paraformaldehyde in PBS for 30 min at 37 °C, permeabilized with PBST for 1 h, stained with phalloidin-AF750 (if desired) for 40 min, and blocked with PBST containing 5% bovine serum albumin (BSA) and 5% goat serum (GS) for 3 h at room temperature. The samples were then incubated with the following primary antibodies, diluted in PBST containing 2.5% BSA and 2.5% GS, on an orbital shaker overnight 4 °C: mouse anti-CD31 (Cell Signaling Technology, 3528T, 1:100) for HUVECs; mouse anti-nestin (Millipore Sigma, MAB5326, 1:600), rabbit anti-Sox2 (Cell Signaling Technology, 230645S, 1:400), rabbit anti-MAP2 (Cell Signaling Technology, 4542S, 1:400), and chicken anti-GFAP (Aves Labs, 87987979, 1:1000) for hNSCs; mouse anti-Pax7 (Developmental Studies Hybridoma Bank, PAX7, 2 μg mL−1), mouse anti-MyoD (Santa Cruz Biotechnology, sc-377460, 1:200), rabbit anti-myogenin (Thermo Fisher Scientific, PA5–110007, 1:400), mouse anti-SAA (Millipore Sigma, A7811, 1:500), and dystrophin (Developmental Studies Hybridoma Bank, MANEX1A(4C7), 2 μg mL−1) for myoblasts. After washing 3 times with PBST at room temperature, the samples were incubated with the appropriate secondary antibodies from Jackson Immuno Research from the following list, diluted in PBST containing 2.5% BSA and 2.5% GS, on an orbital shaker overnight 4 °C: AF647 goat anti-mouse IgG1 (115-605-205, 1:500) for HUVECs; AF647 goat anti-mouse IgG1 (115-605-205, 1:600), Cy3 goat anti-rabbit IgG (111-165-144, 1:400), AF488 goat anti-rabbit IgG (111-545-144, 1:400), and AF647 goat anti-chicken IgY (103-605-155, 1:400) for hNSCs; AF647 goat anti-mouse IgG1 (115-605-205, 1:500), Cy3 goat anti-mouse IgG2b (115-165-207, 1:500), and AF488 goat anti-rabbit IgG (111-545-144, 1:500) for myoblasts. Following 3 additional PBST washes at room temperature, the stained samples were imaged by confocal microscopy.
Mutual Orthogonal Functionalization of Cell-Encapsulating Hydrogels:
Fibroblasts were encapsulated inhNSCs ELP-PEG hydrogels containing excess azides only, excess isonitriles only, or excess azides and isonitriles. The fibroblasts were cultured for 7 d. Fluorescent dyes (Biotium) were diluted in complete maintenance medium to 10 μM. The cell-encapsulating gels were first treated with either CF640R-BCN or the negative control CF640R-NH2 for 1 h at 37 °C. The gels were then washed with fresh maintenance medium (3 × 750 μL) and treated with either CF488A-Tz or the negative control CF488A-NH2 for 2 h at 37 °C. The gels were then washed with fresh maintenance medium (3 × 750 μL), and either fixed with 4% paraformaldehyde in PBS for fluorescence microscopy analysis or digested by incubation with 0.5% trypsin/EDTA for 30 min at 37 °C. The fixed samples were stained with DAPI and phalloidin as described above and imaged by confocal microscopy. For the digestion samples, the mixture was added to a 96 well black bottom plate, and fluorescent intensity was measured using a microplate reader.
Statistical Analysis:
At least 3 independent replicates were used for each experiment. Statistical analysis was performed using GraphPad Prism 10. Comparisons among more than two experimental groups with a single varying parameter were performed using one-way analysis of variance (ANOVA) with Bonferroni post-hoc testing. n.s. = not significant (p>0.05), *p<0.05, **p<0.01, ***p<0.001, ****p<0.0001.
Supplementary Material
Supporting Information is available from the Wiley Online Library.
Acknowledgements
The authors thank Adeola Dosunmu (University of Pennsylvania) for assistance with ELP expression and purification. L.B. is supported by the U.S. National Science Foundation Graduate Research Fellowships Program (GRFP). Funding for this work was provided by the U.S. National Institutes of Health (R00 AG071738 to C.M.M.).
Contributor Information
Ping Zhou, Department of Materials Science & Engineering, University of Pennsylvania, Philadelphia, PA 19104, USA.
Lauren Brown, Department of Bioengineering, University of Pennsylvania, Philadelphia, PA 19104, USA.
Christopher M. Madl, Department of Materials Science & Engineering, University of Pennsylvania, Philadelphia, PA 19104, USA
References
- [1].a) Chaudhuri O, Cooper-White J, Janmey PA, Mooney DJ, Shenoy VB, Nature 2020, 584, 535; [DOI] [PMC free article] [PubMed] [Google Scholar]; b) Yuk H, Wu J, Zhao X, Nat. Rev. Mater 2022, 7, 935; [Google Scholar]; c) Tsou YH, Khoneisser J, Huang PC, Xu X, Bioact. Mater 2016, 1, 39. [DOI] [PMC free article] [PubMed] [Google Scholar]
- [2].a) Lou J, Mooney DJ, Nat. Rev. Chem 2022, 6, 726; [DOI] [PubMed] [Google Scholar]; b) Madl CM, Katz LM, Heilshorn SC, Adv. Funct. Mater 2016, 26, 3612; [DOI] [PMC free article] [PubMed] [Google Scholar]; c) Zhu D, Wang H, Trinh P, Heilshorn SC, Yang F, Biomaterials 2017, 127, 132; [DOI] [PMC free article] [PubMed] [Google Scholar]; d) Tong X, Yang F, Adv. Mater 2016, 28, 7257. [DOI] [PMC free article] [PubMed] [Google Scholar]
- [3].Franzini RM, Deb T, Synlett 2020, 31, 938. [Google Scholar]
- [4].a) La Pierre HS, Arnold J, Bergman RG, Toste FD, Inorg. Chem 2012, 51, 13334; [DOI] [PubMed] [Google Scholar]; b) Massarotti A, Brunelli F, Aprile S, Giustiniano M, Tron GC, Chem. Rev 2021, 121, 10742. [DOI] [PubMed] [Google Scholar]
- [5].Goldstein L, Niv A, Appl. Biochem. Biotechnol 1993, 42. [Google Scholar]
- [6].a) Schäfer RJB, Wilson K, Biedermann M, Moore BS, Sieber S, Wennemers H, Chem. Eur. J 2023, 29, e202203277; [DOI] [PMC free article] [PubMed] [Google Scholar]; b) Huang YB, Cai W, Del Rio Flores A, Twigg FF, Zhang W, Anal. Chem 2020, 92, 599. [DOI] [PMC free article] [PubMed] [Google Scholar]
- [7].a) Antoniazzi G, Schafer RJB, Biedermann M, Ruttimann E, Wennemers H, Chem. Eur. J 2023, 29, e202302389; [DOI] [PubMed] [Google Scholar]; b) Chen Y, Wu KL, Tang J, Loredo A, Clements J, Pei J, Peng Z, Gupta R, Fang X, Xiao H, ACS Chem. Biol 2019, 14, 2793. [DOI] [PMC free article] [PubMed] [Google Scholar]
- [8].Tu J, Xu M, Parvez S, Peterson RT, Franzini RM, J. Am. Chem. Soc 2018, 140, 8410. [DOI] [PubMed] [Google Scholar]
- [9].Markos A, Biedermann M, Heimgärtner J, Schmitt A, Lang K, Wennemers H, J. Am. Chem. Soc 2023, 145, 19513. [DOI] [PubMed] [Google Scholar]
- [10].a) Gu W, Huang J, Lu Y, Lin W, Xu W, Chen FJ, J. Org. Chem 2024, 89, 6364; [DOI] [PubMed] [Google Scholar]; b) Chen Q, Long T, Zheng J, Sheng W, Sun S, Wei W, Zhao J, Wang H, CCS Chem. 2022, 4, 3355. [Google Scholar]
- [11].Schafer RJB, Monaco MR, Li M, Tirla A, Rivera-Fuentes P, Wennemers H, J. Am. Chem. Soc 2019, 141, 18644. [DOI] [PubMed] [Google Scholar]
- [12].a) Truong VX, Zhou K, Simon GP, Forsythe JS, Macromol. Rapid Commun 2015, 36, 1729; [DOI] [PubMed] [Google Scholar]; b) Madl CM, Flaig IA, Holbrook CA, Wang YX, Blau HM, Biomaterials 2021, 275, 120973. [DOI] [PMC free article] [PubMed] [Google Scholar]
- [13].Liu W, Gong X, Zhu Y, Wang J, Ngai T, Wu C, Macromolecules 2019, 52, 8956. [Google Scholar]
- [14].Maj M, Ahn C, Kossowska D, Park K, Kwak K, Han H, Cho M, Phys. Chem. Chem. Phys 2015, 17, 11770. [DOI] [PubMed] [Google Scholar]
- [15].Stockmann H, Neves AA, Stairs S, Brindle KM, Leeper FJ, Org. Biomol. Chem 2011, 9, 7303. [DOI] [PubMed] [Google Scholar]
- [16].(a) Kopyeva I, Goldner EC, Hoye JW, Yang S, Regier MC, Bradford JC, Vera KR, Bretherton RC, Robinson JL, DeForest CA, Adv. Mater 2024, 36, 2404880; [DOI] [PMC free article] [PubMed] [Google Scholar]; b) Roth JG, Huang MS, Navarro RS, Akram JT, LeSavage BL, Heilshorn SC, Sci. Adv 2023, 9, eadh8313; [DOI] [PMC free article] [PubMed] [Google Scholar]; c) Chaudhuri O, Gu L, Klumpers D, Darnell M, Bencherif SA, Weaver JC, Huebsch N, Lee HP, Lippens E, Duda GN, Mooney DJ, Nat. Mater 2016, 15, 326. [DOI] [PMC free article] [PubMed] [Google Scholar]
- [17].Madl CM, Katz LM, Heilshorn SC, ACS Macro Lett. 2018, 7, 1302. [DOI] [PMC free article] [PubMed] [Google Scholar]
- [18].Straley KS, Heilshorn SC, Soft Matter 2009, 5, 114. [Google Scholar]
- [19].a) Song HG, Rumma RT, Ozaki CK, Edelman ER, Chen CS, Cell Stem Cell 2018, 22, 340; [DOI] [PMC free article] [PubMed] [Google Scholar]; b) Jain RK, Au P, Tam J, Duda DG, Fukumura D, Nat. Biotechnol 2005, 23, 821. [DOI] [PubMed] [Google Scholar]
- [20].a) Madl CM, Heilshorn SC, Annu. Rev. Biomed. Eng 2018, 20, 21; [DOI] [PMC free article] [PubMed] [Google Scholar]; b) Madl CM, LeSavage BL, Dewi RE, Dinh CB, Stowers RS, Khariton M, Lampe KJ, Nguyen D, Chaudhuri O, Enejder A, Heilshorn SC, Nat. Mater 2017, 16, 1233. [DOI] [PMC free article] [PubMed] [Google Scholar]
- [21].Liu J, Saul D, Boker KO, Ernst J, Lehman W, Schilling AF, Biomed Res. Int 2018, 2018, 1984879. [DOI] [PMC free article] [PubMed] [Google Scholar]
- [22].Shen BQ, Xu K, Liu L, Raab H, Bhakta S, Kenrick M, Parsons-Reponte KL, Tien J, Yu SF, Mai E, Li D, Tibbitts J, Baudys J, Saad OM, Scales SJ, McDonald PJ, Hass PE, Eigenbrot C, Nguyen T, Solis WA, Fuji RN, Flagella KM, Patel D, Spencer SD, Khawli LA, Ebens A, Wong WL, Vandlen R, Kaur S, Sliwkowski MX, Scheller RH, Polakis P, Junutula JR, Nat. Biotechnol 2012, 30, 184. [DOI] [PubMed] [Google Scholar]
- [23].Madl CM, Heilshorn SC, Adv. Funct. Mater 2018, 28, 1706046. [DOI] [PMC free article] [PubMed] [Google Scholar]
- [24].Jiang Y, Chen J, Deng C, Suuronen EJ, Zhong Z, Biomaterials 2014, 35, 4969. [DOI] [PubMed] [Google Scholar]
- [25].Scinto SL, Bilodeau DA, Hincapie R, Lee W, Nguyen SS, Xu M, Am Ende CW, Finn MG, Lang K, Lin Q, Pezacki JP, Prescher JA, Robillard MS, Fox JM, Nat. Rev. Methods Primers 1, 2021, 30. [DOI] [PMC free article] [PubMed] [Google Scholar]
- [26].a) Xu M, Deb T, Tu J, Franzini RM, J. Org. Chem 2019, 84, 15520; [DOI] [PubMed] [Google Scholar]; b) Stairs S, Neves AA, Stockmann H, Wainman YA, Ireland-Zecchini H, Brindle KM, Leeper FJ, Chembiochem 2013, 14, 1063. [DOI] [PMC free article] [PubMed] [Google Scholar]
- [27].Rapp TL, DeForest CA, Adv. Healthcare. Mater 2020, 9, e1901553. [DOI] [PubMed] [Google Scholar]
- [28].a) Cambria E, Renggli K, Ahrens CC, Cook CD, Kroll C, Krueger AT, Imperiali B, Griffith LG, Biomacromolecules 2015, 16, 2316; [DOI] [PMC free article] [PubMed] [Google Scholar]; b) Bretherton RC, Haack AJ, Kopyeva I, Rahman F, Kern JD, Bugg D, Theberge AB, Davis J, DeForest CA, Adv. Mater 2023, 35, e2209904. [DOI] [PMC free article] [PubMed] [Google Scholar]
- [29].Chang PV, Prescher JA, Sletten EM, Baskin JM, Miller IA, Agard NJ, Lo A, Bertozzi CR, Proc. Natl. Acad. Sci. U. S. A 2010, 107, 1821. [DOI] [PMC free article] [PubMed] [Google Scholar]
- [30].Brudno Y, Desai RM, Kwee BJ, Joshi NS, Aizenberg M, Mooney DJ, ChemMedChem 2015, 10, 617. [DOI] [PubMed] [Google Scholar]
- [31].DeForest CA, Tirrell DA, Nat. Mater 2015, 14, 523. [DOI] [PubMed] [Google Scholar]
- [32].Shilling PJ, Mirzadeh K, Cumming AJ, Widesheim M, Kock Z, Daley DO, Commun. Biol 2020, 3, 214. [DOI] [PMC free article] [PubMed] [Google Scholar]
- [33].LeSavage BL, Suhar NA, Madl CM, Heilshorn SC, J. Vis. Exp 2018, 135. E57739. [DOI] [PMC free article] [PubMed] [Google Scholar]
Associated Data
This section collects any data citations, data availability statements, or supplementary materials included in this article.