Skip to main content
. 2025 Aug 12;15(35):28601–28612. doi: 10.1039/d5ra04501k

Table 3. Catalytic evaluation at different temperatures using Ni1/Et2AlCl for ethylene polymerizationa.

Entry T/°C Activityb M w c M w/Mnc T m d
1 20 4.67 10.90 6.81 55.40
2 30 4.27 9.02 3.38 41.18
3 40 4.07 6.57 2.29 39.62
4 50 3.82 5.29 2.19 15.94
5 70 3.20 5.15 1.72 e
6 80 2.92 4.64 2.23 e
7 90 2.56 2.67 1.21 e
a

Conditions: 2 μmol Ni1 and 100 mL toluene, 10 atm C2H4, 30 min, Al/Ni = 600.

b

106 g(PE) mol−1 (Ni) h−1.

c

M w: 105 g mol−1, Mw and Mw/Mn determined by GPC.

d

Determined by DSC.

e

Broad and weak endotherms, amorphous-like polyethylenes.