Table 5. Cone calorimeter test data of PP and its flame-retardant composites.
| Sample | TTI [s] | PHRR [kW m−2] | t PHRR [s] | THR [MJ m−2] | FPI [s m2 kW−1] | FGI [kW (m−2 s−1)] | TSR [m2 m−2] |
|---|---|---|---|---|---|---|---|
| PP | 43 | 978.5 | 200 | 150.5 | 0.044 | 4.89 | 1451.4 |
| P1 | 34 | 309.8 | 73 | 109.8 | 0.109 | 4.24 | 454.7 |
| P2 | 27 | 255.8 | 71 | 113.8 | 0.106 | 3.60 | 769.6 |
| P6 | 29 | 251.1 | 65 | 121.9 | 0.115 | 3.86 | 233.3 |