Skip to main content
ACS Omega logoLink to ACS Omega
. 2025 Sep 25;10(39):45767–45777. doi: 10.1021/acsomega.5c06243

Enhancing Performance of Silica-Filled Isoprene Rubber: The Synergistic Role of Urea and Silane Coupling Agent

Naratip Chuma †, Wannarat Chueangchayaphan †, Keisuke Chino ‡, Jutharat Intapun †,*
PMCID: PMC12508995  PMID: 41078742

Abstract

This study investigated the compatibility between silica and synthetic polyisoprene rubber (IR) by examining the synergistic effects of urea and silane (Si-75) as coupling agents. Comparative analyses were conducted on synthetic IR formulations containing silica: without silane (Si-75), with silane alone, and with a combination of silane (Si-75) and urea. The results revealed that the presence of urea alongside silane reduced both cure and scorch times while increasing maximum and delta torques. These findings suggest an enhanced interaction between synthetic IR and the amine groups of urea on the silica surface. Furthermore, the combination of urea and Si-75 enhanced the 100% and 300% modulus, as well as the tensile strength of vulcanized IR. Analyses of the Payne effect, cross-link density, and FTIR confirmed a more effective distribution of silica within the IR matrix. Scanning electron microscopy characterization revealed smaller silica agglomerates in the IR/silane/urea system. Dynamic mechanical analysis provided a comprehensive evaluation, corroborating that urea, in conjunction with silane, facilitates optimal silica dispersion in the IR.


graphic file with name ao5c06243_0011.jpg


graphic file with name ao5c06243_0009.jpg

1. Introduction

The automotive industry’s relentless pursuit of sustainability has catalyzed the development of “green tire” technology, which prioritizes environmental stewardship throughout the entire tire lifecycle from manufacturing to disposal. To meet the growing demand for high-performance automotive tires, modern green tire production increasingly relies on silica (Si) fillers. This technology helps reduce fuel consumption and support environmental protection by lowering the tire’s rolling resistance. A notable shift has occurred in the tire industry, where Si has emerged as a sustainable and technologically superior alternative to conventional carbon black. Its incorporation not only reduces rolling resistance, contributing to lower fuel consumption and CO2 emissions. Consequently, the development of Si-reinforced green tires represents a critical intersection of material innovation, environmental sustainability, and industrial performance optimization. Despite its environmental and performance advantages, Si incorporation presents formidable technical challenges that have hindered its widespread adoption. The primary obstacle stems from Si’s inherent tendency to absorb vulcanization accelerators, thereby impeding cross-linking reactions and compromising cure efficiency. Furthermore, the polar nature of silanol groups (Si–OH) on Si surfaces promotes extensive filler–filler interactions, resulting in large agglomerate formation that creates stress concentration points and weakens the overall composite structure. This agglomeration phenomenon severely limits stress transfer efficiency during deformation and creates incompatibility with the hydrophobic rubber matrix. To address these challenges, it has extensively employed silane coupling agents as molecular bridges, facilitating condensation reactions between alkoxy functional groups (such as methoxy –OCH3 or ethoxy –OC2H5) in silanes and surface silanol groups on Si particles. These reactions generate stable siloxane bridges (Si–O–Si), effectively reducing silanol reactivity and promoting superior Si dispersion within the rubber matrix. , The silane-mediated surface modification strategy has proven to be successful in enhancing Si–elastomer interactions while simultaneously minimizing detrimental filler–filler networks. Recent research endeavors have explored innovative approaches to optimize Si-rubber compatibility beyond conventional silane systems. Notable investigations include the application of liquid polybutadiene to enhance Si/silane system compatibility in tire compounds and the utilization of 1-ethyl-3-methylimidazolium acetate ionic liquid as a volatile organic compound-free alternative to silane in NBR vulcanizate nanocomposites, resulting in improved dispersion, increased bound rubber content, and enhanced cross-link density. Additionally, cardanol-grafted liquid isoprene rubber (CA-g-LIR) with branched architecture has been successfully employed to strengthen interfacial adhesion between SiO2 and natural rubber (NR), while specialized coupling agents such as 2-aminoethyl-2-(3-triethoxysilylpropyl)­aminoethyl disulfide (ATD) have shown promise in developing Si-based rubber composites with superior mechanical properties and reduced hysteresis. The application of Si reinforcement has been extensively studied across diverse rubber matrices, including NR, deproteinized NR, styrene–butadiene rubber (SBR), ethylene propylene diene monomer rubber (EPDM), and synthetic IR. , However, IR presents unique challenges due to its purely hydrocarbon structure, which lacks the nonrubber constituents that typically facilitate silanization reactions in NR systems. The significant polarity mismatch and solubility parameter differences between hydrophobic IR chains and polar Si surfaces exacerbate filler aggregation tendencies, making effective Si dispersion particularly challenging and often resulting in compromised mechanical properties. While silane coupling agents remain the predominant surface treatment approach, their high cost and potential interference with vulcanization kinetics necessitate the exploration of alternative, more economically viable solutions.

Urea has emerged as a promising and underexplored alternative that addresses both economic and environmental concerns in Si-reinforced rubber technology. This cost-effective, environmentally benign compound possesses unique characteristics that make it particularly attractive for rubber applications. Urea’s exceptional hydrogen bonding capability, attributed to its small polar molecular structure, enables strong interactions with silanol groups on Si surfaces––a mechanism that could potentially reduce filler–filler interactions and promote improved dispersion in rubber matrices. Recent breakthrough research has demonstrated urea’s effectiveness when incorporated as deep eutectic solvents in Si-filled SBR systems, where its hydrogen bonding capacity enhanced both the curing process and Si dispersion. The industrial relevance of urea extends beyond its role as a dispersing aid. Historically utilized in rubber technology for protein removal in NR latex and as a vulcanization accelerator additive, urea’s low molecular weight and polar nature position it as an ideal compatibilizer that can enhance filler–matrix interactions without significantly increasing compound viscosity or disrupting cure kinetics. While ethylene thiourea (ETU) derivatives have been investigated for their vulcanization and mechanical property effects in Si-reinforced rubber blends, comprehensive studies examining urea’s direct role in enhancing Si dispersion in synthetic IR remain remarkably limited, representing a significant knowledge gap in the field. This study addresses this critical research gap by systematically investigating the synergistic effects of urea as both a Si surface modifier and a silanization accelerator in Si-filled IR composites. The research comprehensively evaluates cure characteristics, bound rubber formation, cross-link density, and mechanical properties, including tensile strength, elongation at break, and stress–strain behavior at 100% and 300% elongations. Advanced characterization techniques, including scanning electron microscopy (SEM) for morphological analysis, Fourier transform infrared spectroscopy (FTIR) for chemical interaction assessment, and dynamic mechanical analysis (DMA) for viscoelastic property evaluation, provide comprehensive insights into the underlying mechanisms. The findings contribute to advancing sustainable tire technology by demonstrating how urea-based systems can deliver enhanced performance while offering cost-effective and environmentally responsible alternatives to conventional silane coupling agents in synthetic rubber applications.

2. Experimental Section

2.1. Materials

Synthetic polyisoprene rubber (IR) was purchased from Neo Plastomer Co., Ltd. (Bangkok, Thailand). Silica Ultrasil VN3 grade with a CTAB of 165 m2/g was produced by Evonik Industries AG Ltd. (Essen, Germany), the silane coupling agent, bis­(triethoxysilylpropyl) disulfide (Si-75), was purchased from Sigma-Aldrich (St. Louis, USA), and urea was purchased from Sigma (St. Louis, USA). The additives, namely, zinc oxide (ZnO), stearic acid (SA) (activators), N-(1,3-dimethylbutyl)-N′-phenyl-p-phenylenediamine (6PPD) (antioxidant), N-cyclohexyl-2-benzothiazole sulfenamide (CBS), 1,3-diphenylguanidine (DPG) (accelerators), and sulfur curing agent, were provided by Ajax Chemical Co., Ltd. (Samut Sakhon, Thailand).

2.2. Compounding of Isoprene Rubber with Silica, Urea, and Silane

The rubber formulations employed in this investigation are listed in Table . A two-stage mixing process was utilized in the preparation of the rubber compounds, as shown in Table . In the initial stage, mixing was conducted using an internal Brabender Plasti-Corder model 50 EHT, 835205 (Duisburg, Germany), at 60 °C and a rotor speed of 60 rpm. A rubber masterbatch was prepared by initially mixing a portion of the Si with urea, ZnO, SA, and 6PPD. The remaining Si was then added along with Si-75, and the mixing process continued for 8 min. The rotor speed was maintained at 60 rpm with a fill factor of 0.75 (75%) and a temperature setting of 150 °C. In the second stage, the curatives (DPG, CBS, and sulfur) were sequentially added to the mixture, and mixing was continued at a rotor speed of 30 rpm with the temperature maintained at 40 °C.

1. Formulation of Silica-Filled Polyisoprene Rubber Composites.

  contents (phr)
ingredient IR IR-Si IR-Si/Urea IR-Si/Si-75 IR-Si/Si-75/Urea
isoprene rubber (IR) 100 100 100 100 100
silica (Si)   40 40 40 40
zinc oxide 3 3 3 3 3
stearic acid 1 1 1 1 1
6PPD 1 1 1 1 1
Si-75       3.2 3.2
urea     1 1 1
CBS 1 1 1 1 1
DPG 0.5 0.5 0.5 0.5 0.5
sulfur 2 2 2 2 2

2. Two-Step Mixing Procedure for Preparing Silica-Filled Polyisoprene Rubber Composite.

stage time (min) mixing procedure temperature (°C)
1st stage 0:00 add rubber (preheated to 60 °C) 150
  1:00 add half of the silica along with urea, ZnO, SA, and 6PPD  
  2:50 add the remaining silica and Si-75  
  4:00 operate ram up and down  
  5:00 repeat ram up and down again  
  8:00 discharge  
2nd stage 0:00 add the masterbatch from the first stage 40
  1:00 add CBS and DPG  
  2:00 add sulfur  
  3:00 discharge  

2.3. Vulcanization of Silica-Filled Polyisoprene Rubber

Compression molding was performed using a PR1DW400L450PM press, Charoen That Co., Ltd. (Bangkok, Thailand), to prepare vulcanized IR sheets at 150 °C, based on curing times determined by rheometer tests.

2.4. Cure Characterization

The cure characteristics of the rubber compounds were evaluated at 150 °C by using a moving die rheometer, Alpha Technologies (Ohio, USA), operating at a fixed frequency of 1.67 Hz and a strain amplitude of 1° arc. Key parameters, including optimum scorch time (t s1), cure time (t c90), minimum torque (M L), maximum torque (M H), and torque difference or delta torque (M H –M L), were obtained from the curing curves.

2.5. Payne Effect

Filler–filler interactions in the compound samples were evaluated using a rubber processing analyzer, RPA 2000, Alpha Technologies (Ohio, USA). The test involved measuring the storage shear modulus (G′) of each unvulcanized, Si-filled rubber compound under shear deformation across a strain amplitude range of 0.56–100%, at the fixed oscillating frequency of 1 Hz and at a test temperature 100 °C. The Payne effect was quantified as the change in storage modulus (ΔG′) in a wide range of strain deformation, calculated by subtracting the G′ value at the maximum strain amplitude (100%) from that at the minimum strain (0.56%). This difference represents the Payne effect and reflects the degree of filler–filler interactions within the compound.

2.6. Bound Rubber Content and Cross-Link Density

The bound rubber content of the Si-filled IR composite was determined using the swelling method. Initially, rubber compounds of various formulations were cut into small pieces, placed in stainless steel cages, and accurately weighed. The cages were then immersed in 20 mL of toluene for 72 h at ambient temperature, with the solvent being replaced every 24 h. After the swelling period, the cages were removed and dried in a hot-air oven at 105 °C for 24 h. The bound rubber content was subsequently calculated by the following eq .

Boundrubbercontent(%)=(Wfg−Wf)Wp 1

where W f and W p represent the weights of the filler and rubber in the specimens, respectively, while W fg denotes the weight of filler with bound rubber remaining after toluene extraction.

Equilibrium swelling measurements were conducted to determine the cross-link density of Si-filled IR composites. This method relies on the characteristic volumetric expansion of a cross-linked rubber network when immersed in a suitable solvent. Solvent molecules penetrate the network, diffusing between the interconnected rubber chains and causing significant swelling. Vulcanized rubber specimens, measuring 10 × 10 × 2 mm3, were initially weighed and then immersed in toluene at ambient temperature for 7 days. After swelling, the samples were removed, and excess solvent was carefully blotted from the surfaces using filter paper. The specimens were then dried in a vacuum oven at 40 °C for 24 h. The samples were then weighed, dried, and weighed again. The cross-link density of the vulcanizates was subsequently calculated usingaccording to the Flory–Rehner equation (eq ).

Vc={−(ln(1−Vr)+Vr+χ*Vr2)}Vs(Vr1/3−Vr2) 2

where V s represents the molecular volume of the solvent (106.2 cm3/mol). χ* is the Flory–Huggins interaction parameter between toluene and rubber, with a value of 0.397.

In this context, V r denotes the volume fraction of polymer in the swollen rubber within the pure solvent and is calculated using eq .

1Vr=1+W1ρrW2ρs 3

where W 1 and W 2 are the weights (g) of the sample before and after immersion in toluene, respectively, ρr and ρs represent the densities of the rubber (0.92 g/cm3) and solvent (0.87 g/cm3), respectively. Additionally, all reported values represent the average of three replicates.

2.7. Mechanical Properties

Tensile tests were conducted using a Tinius Olsen model 10ST tensiometer (Salfords, England), at a crosshead speed of 500 mm/min, in accordance with ISO 527 standards. Dumbbell-shaped samples, conforming to ISO 527 Type B, were prepared to evaluate the stress–strain behavior, including 100% modulus (M 100), 300% modulus (M 300), tensile strength, and elongation at break of the Si-filled IR. To investigate the relationship between the chemical bonding of IR and the Si filler, the reinforcement index was evaluated based on the modulus ratio M 300/M 100. The specimens were cut into Type B dumbbell shapes from compression-molded rubber sheets of each formulation. A total of five specimens were tested for each formulation.

2.8. Fourier Transform Infrared Spectroscopy

FTIR was employed to analyze the chemical functional groups of the samples in the attenuated total reflectance mode. This technique measures the infrared absorption spectrum of a vulcanized IR sample. Spectral data were collected over a wavelength range of 400–4000 cm–1, with 32 scans per spectrum at a resolution of 2 cm–1. The instrument used was a Spectrum Two model from PerkinElmer (Waltham, Massachusetts, USA).

2.9. Scanning Electron Microscopy

SEM was employed to examine the surface topology and filler distribution of Si within the IR matrix. A Zeiss Supra-40 VP SEM (Carl Zeiss Microscopy GmbH, Oberkochen, Germany) was utilized, operating at a 1000× magnification. Samples with fresh cross-sections were prepared by cryogenic fracturing in liquid nitrogen to preserve their morphology. Prior to SEM analysis, the samples were sputter-coated with a gold layer to enhance electrical conductivity.

2.10. Dynamic Mechanical Analysis

The storage and loss moduli of IR composites were evaluated over a temperature range of −80 to 100 °C, at a heating rate of 5 °C/min and a frequency of 1 Hz. Liquid nitrogen was employed as the refrigerant. The analysis was conducted using a PerkinElmer DMA 8000 instrument (PerkinElmer Inc., Waltham, USA).

3. Results and Discussion

3.1. Cure Characteristics

Figure presents the curing time profiles and torque development for Si-filled IR compounds containing urea with and without silane (Si-75). The fundamental cure parameters, minimum torque (M L), maximum torque (M H), scorch time (t s2 ), cure time (t c90), and cure rate index (CRI) provided critical insights into the vulcanization behavior and cross-linking efficiency of these formulations. While Table presents the cure characteristic values of Si-filled IR formulations.

1.

1

Cure characteristic of silica-filled polyisoprene composites.

3. Cure Characteristics of Silica-Filled-Polyisoprene Rubber Compounds.

  cure characteristics
sample cure time (t c90) (min) scorch time (t s1) (min) cure rate index (CRI) (min–1) minimum torque (M L) (dN m) maximum torque (M H) (dN m) torque difference (M H – M L) (dN m)
IR 8.4 ± 0.4 1.2 ± 0.2 13.9 ± 0.1 1.4 ± 0.4 11.9 ± 1.3 10.5 ± 0.2
IR-Si 13.2 ± 0.7 1.4 ± 0.3 8.4 ± 0.2 4.6 ± 0.6 17.4 ± 0.7 12.8 ± 0.2
IR-Si/urea 8.3 ± 0.9 1.0 ± 0.7 13.7 ± 0.3 8.8 ± 0.2 25.0 ± 0.5 16.2 ± 0.6
IR-Si/Si-75 10.4 ± 1.1 1.2 ± 0.4 10.8 ± 0.2 5.0 ± 0.4 21.3 ± 1.1 16.3 ± 0.4
IR-Si/Si-75/urea 8.9 ± 0.8 1.2 ± 0.2 13.0 ± 0.3 8.3 ± 0.8 28.6 ± 0.4 20.4 ± 0.7

The neat IR formulation exhibited the lowest torque levels, establishing the baseline mechanical properties without filler reinforcement. Upon Si incorporation (IR-Si), a notable increase in both M L and M H values was observed, primarily attributed to the inherent stiffness of Si agglomerates and the formation of extensive filler–filler networks within the matrix.

The introduction of urea as a surface modifier dramatically altered the cure behavior. Formulations containing urea without silane (IR-Si/urea) demonstrated significantly enhanced minimum torque, maximum torque, and torque difference compared to the Si-only system. This improvement is attributed to urea’s unique ability to form hydrogen bonds with silanol groups through its amine functionality (–NH2), effectively neutralizing surface acidity and reducing the absorption of curing agents. Consequently, the CRI increased substantially, approaching levels comparable to those of silane-treated systems. The torque difference (M H – M L) serves as a direct indicator of cross-link density, minimum torque (M L) is a crucial indicator of the viscosity, directly reflecting the flow behavior of IR-Si/urea during processing, while M H reflects the final stiffness of the vulcanized compound. ,

Silane-containing formulations (IR-Si/Si-75) showed expected improvements in both maximum torque and torque difference, confirming the effectiveness of silanization in promoting Si-rubber interactions through the formation of stable siloxane bridges (Si–O–Si). The alkoxy groups of Si-75 react with surface silanol groups during mixing, reducing filler–filler interactions and enhancing dispersion within the rubber matrix.

The synergistic effect became most pronounced when urea and Si-75 were combined. The IR-Si/urea/Si-75 formulation achieved the highest maximum torque and torque difference, exceeding the performance of the individual additives. This synergistic enhancement can be attributed to urea’s dual role: (1) as a surface coating agent that improves Si dispersion, and (2) as a silanization accelerator that promotes the condensation reaction between silane and Si through its amine groups. The enhanced silanization efficiency results in superior cross-linking, as evidenced by the highest M H –M L values observed in this formulation. This improved dispersion minimizes catalyst absorption, thereby promoting more efficient vulcanization reactions and reducing the cure time (t c90).

3.2. The Payne Effect

The Payne effect, characterized by strain-dependent reduction in storage modulus and accompanying maximum in loss modulus, provides crucial information about filler–filler interactions and network structure in filled rubber systems. Figure a illustrates the storage modulus behavior as a function of strain amplitude for Si-filled IR composites with different coupling agent systems.

2.

2

(a) Storage modulus as a function of strain amplitude and (b) storage modulus difference, indicating the Payne effect of silica-filled polyisoprene rubber composites.

The IR-Si composite exhibited the most pronounced Payne effect, indicating the strongest filler–filler interactions among all tested formulations. This behavior correlates directly with the large Si agglomerates observed in the SEM micrographs (Figure a), confirming poor dispersion and extensive secondary structure formation. The high storage modulus difference (Figure b) reflects the presence of a percolating filler network that breaks down under an increasing strain.

5.

5

SEM micrographs showing the surface topologies of silica-filled IR composites.

Urea incorporation significantly reduced the magnitude of the Payne effect. The IR-Si/urea composite showed substantially lower storage modulus differences compared to the untreated Si system, indicating reduced filler–filler interactions. This improvement is attributed to urea’s hydrogen bonding capability with silanol groups, which disrupts the formation of Si aggregates and promotes better dispersion within the IR matrix. The reduction in the Payne effect directly correlates with the enhanced cure characteristics observed in Section , demonstrating the interconnected nature of the dispersion quality and vulcanization efficiency.

The combination of urea and silane resulted in the lowest Payne effect, confirming optimal filler dispersion and minimal filler–filler interactions. This finding supports the synergistic mechanism proposed earlier, where urea facilitates initial dispersion, while silane provides chemical coupling between the filler and rubber matrix.

3.3. Bound Rubber Content and Cross-Link Density

The bound rubber content, representing rubber chains that are chemically bonded or physically entrapped within the filler network, serves as a sensitive indicator of filler–rubber interactions. Figure demonstrates the progressive enhancement of bound rubber content across different formulations, directly correlating with the cure characteristic improvements discussed previously.

3.

3

Bound rubber content and cross-link density.

The neat IR formulation exhibited minimal bound rubber content, confirming the absence of reinforcing interactions. Si addition resulted in a modest increase, primarily due to physical entrapment rather than strong chemical interactions. The addition of urea produced a more substantial increase in the bound rubber content, supporting the proposed mechanism of enhanced filler–rubber interactions through hydrogen bonding. The amine groups in urea effectively coat the polar Si surfaces, creating a more compatible interface that promotes rubber chain adsorption and entanglement.

The highest bound rubber content was achieved with the combined urea-silane system, consistent with the superior cure characteristics and reduced Payne effect observed in this formulation. This finding indicates that urea not only improves the initial Si dispersion but also enhances the efficiency of subsequent silanization reactions, leading to stronger chemical bonds between the filler and rubber matrix.

Cross-link density measurements (Figure ) revealed parallel trends with bound rubber content, confirming the mechanistic relationship between filler–rubber interactions and network formation. The formulation without Si exhibited the lowest cross-link density, while Si addition produced a slight increase. Urea incorporation resulted in more substantial enhancement, and the combination with silane achieved the highest cross-link density.

The enhanced cross-link density in urea-containing formulations can be attributed to the dual role of amine groups: (1) improving Si dispersion through surface coating, which increases the effective surface area available for rubber–filler interactions, and (2) accelerating silanization reactions, which promote the formation of covalent bonds between silane coupling agents and the rubber matrix. This improved cross-linking efficiency directly translates to superior mechanical properties, as will be demonstrated in the stress–strain analysis (Table ).

4. Mechanical Properties of Silica-Filled Isoprene Rubber Composite.

  mechanical properties of the vulcanizates
samples modulus 100% modulus 300% reinforcement index tensile strength (MPa) elongation at break (%)
IR 1.1 ± 0.3 2.5 ± 0.6 2.3 ± 0.2 9.5 ± 0.8 553 ± 11
IR-Si 1.1 ± 0.5 2.7 ± 0.4 2.5 ± 0.1 10.5 ± 1.0 543 ± 8
IR-Si/urea 1.8 ± 0.4 4.7 ± 0.7 2.6 ± 0.3 15.2 ± 1.4 524 ± 9
IR-Si/Si-75 1.9 ± 0.6 3.9 ± 0.7 2.0 ± 0.6 13.5 ± 1.2 513 ± 11
IR-Si/Si75/urea 1.8 ± 0.5 4.9 ± 0.6 2.7 ± 0.5 16.7 ± 1.3 534 ± 11

The interconnected nature of these results demonstrates a clear structure–property relationship: improved Si dispersion (reduced Payne effect) leads to enhanced filler–rubber interactions (increased bound rubber), which promotes more efficient cross-linking (higher cross-link density), ultimately resulting in superior cure characteristics and mechanical performance. The synergistic combination of urea and silane optimizes each step of this process, validating the proposed dual-mechanism approach for enhancing Si-filled IR composites.

3.4. Mechanical Properties of the Vulcanizates

The mechanical properties of vulcanized rubber composites serve as the ultimate validation of the structure–property relationships established through cure characteristics, Payne effect analysis, and cross-link density measurements. Table presents the comprehensive mechanical performance data, including tensile strength, elongation at break, 100% modulus, and 300% modulus, demonstrating how the enhanced cross-linking efficiency translates into superior practical performance.

The neat IR formulation exhibited the poorest mechanical properties, confirming the absence of the reinforcing mechanisms typically associated with strain-induced crystallization in NR systems. This baseline performance highlights the inherent limitations of synthetic IR and underscores the critical importance of effective filler reinforcement. ,

Si incorporation alone provided modest improvements in both stress and tensile strength, which is attributed to the inherent stiffness of Si particles. However, the benefits were limited by poor dispersion and extensive filler–filler interactions, as evidenced by the high Payne effect observed in Section . The formation of large agglomerates created stress concentration points that compromised the overall reinforcing efficiency.

Urea addition produced remarkable mechanical property enhancements that directly correlate with the improved dispersion and cross-linking characteristics discussed previously. The IR-Si/urea formulation demonstrated substantial increases in both 100% and 300% moduli, indicating enhanced stiffness and load-bearing capacity. This improvement validates the proposed mechanism where urea’s hydrogen bonding capability reduces Si surface acidity, prevents particle agglomeration, and creates a compatible interface that promotes effective stress transfer from the rubber matrix to the filler particles.

The silane-treated formulation (IR-Si/Si-75) showed the expected improvements in mechanical properties, confirming the effectiveness of chemical coupling through siloxane bridge formation. The enhanced 100% modulus particularly reflects the degree of vulcanization improvement, as silane facilitates better Si dispersion and reduces catalyst absorption during curing. The formation of covalent bonds between Si surfaces and rubber chains creates an efficient stress transfer network that maximizes the reinforcing potential of the filler.

The synergistic combination of urea and silane achieved the highest mechanical performance and reinforcement index of individual additives. The reinforcement index rises with chemically bonded rubber, where the dominant factor is the polymer–filler interfacial area. This superior performance can be attributed to the dual-mechanism enhancement: urea accelerates silanization reactions through its amine functionality while simultaneously improving the initial Si dispersion. The amino groups act as catalytic sites that promote silane condensation reactions, leading to more extensive and efficient chemical coupling. Consequently, the reduced elongation at break reflects the formation of a more tightly cross-linked network with restricted polymer chain mobility. Figure illustrates the stress–strain behavior, revealing that the IR-Si/Si75/urea formulation exhibited the steepest initial slope, indicating the maximum stiffness and toughness. This behavior directly correlates with the highest cross-link density measured in Section , confirming that the enhanced network structure translates into superior load-bearing capacity and energy dissipation characteristics. The improved stress transfer and strain distribution throughout the matrix enhances the composite’s resistance to failure and overall mechanical resilience (Figure a).

4.

4

Stress–strain behaviors of silica-filled polyisoprene composite.

3.5. Morphological Properties

SEM analysis provides crucial visual evidence that validates the structure–property relationships established through mechanical testing and dynamic analysis. Figure demonstrates how the morphological changes induced by urea and silane additions directly correlate with the enhanced mechanical properties and reduced Payne effects discussed in previous sections.

The IR-Si formulation without additives (Figure a) exhibited severe Si agglomeration with large, interconnected clusters that create the percolating network responsible for the pronounced Payne effect observed in Section . This poor dispersion results from the fundamental incompatibility between hydrophilic Si surfaces and the hydrophobic IR matrix, exacerbated by strong silanol–silanol hydrogen bonding that promotes particle–particle interactions.

Urea incorporation (Figure b) produced a dramatic improvement in dispersion quality with significantly smaller and more uniformly distributed Si particles. This morphological enhancement directly explains the reduced Payne effect and improved mechanical properties observed in the IR-Si-urea formulation. The mechanism involves hydrogen bonding between urea’s amine groups and Si’s silanol groups, effectively disrupting the filler–filler interaction network and creating a more compatible filler–matrix interface.

The silane-treated formulation (Figure c) showed comparable dispersion improvement with smaller agglomerates similar to those observed with urea treatment. This confirms that both additives address the fundamental dispersion challenge through different but complementary mechanisms. Silane functions through chemical surface modification via silanization reactions, while urea operates through physical surface coating and hydrogen bonding interactions.

The combined urea-silane system (Figure d) achieved the finest dispersion, with the smallest agglomerate sizes and the most uniform distribution throughout the IR matrix. This superior morphology directly correlates with the highest mechanical properties, lowest Payne effect, and maximum cross-link density observed in this formulation. The enhanced dispersion validates the proposed synergistic mechanism where urea facilitates initial particle separation and subsequently accelerates silane condensation reactions.

The morphological evidence strongly supports the catalytic role of urea in promoting the silanization efficiency. The amine groups adsorb onto Si surfaces, reducing surface energy and filler–filler interactions while simultaneously creating reactive sites that enhance silane coupling reactions. This dual functionality explains why the combined system outperforms individual additives, providing both improved initial dispersion and more efficient chemical coupling.

The morphological analysis confirms the structure–property correlation established throughout this study: optimal Si dispersion (finest particle distribution) leads to minimal filler–filler interactions (reduced Payne effect), enhanced filler–rubber coupling (higher bound rubber and cross-link density), and superior mechanical performance (maximum tensile properties). The visual evidence provided by SEM analysis validates the proposed dual-mechanism approach and demonstrates the practical benefits of the urea-silane synergistic system for advanced rubber composite applications.

3.6. Fourier Transform Infrared Spectroscopy

Figure presents the comparative FTIR spectra of neat IR and various Si-filled formulations, revealing the specific molecular interactions that drive the synergistic effects of urea and silane coupling agents. The neat IR spectrum exhibits characteristic absorption bands at 2920–2850 cm–1 (CH2 stretching), 1641 cm–1 (CC stretching), 1446–1375 cm–1 (CH2, CH3 bending), and 833 cm–1 (C–H bending vibrations in cis-1,4-isoprene units), establishing the baseline polymer fingerprint. Upon Si incorporation (IR-Si), new absorption bands emerge at 3270 cm–1 (O–H stretching of silanol groups) and 1075–1035 cm–1 (Si–O–C vibrations), confirming the presence of reactive silanol functionalities on the filler surface.

6.

6

FTIR spectra of neat composites, including formulations without silane, with silane, and with a combination of urea and silane as coupling agents.

The IR-Si-urea spectrum reveals critical molecular interactions that explain the enhanced dispersion and mechanical properties observed in previous sections. New absorption peaks appear at 3340 cm–1 (N–H stretching), vibration of the urea group is its carbonyl stretching (1624 cm–1), 1545 cm–1 (N–H, C–N stretching), and an observed small peak of 692–692 cm–1 (N–H), confirming urea incorporation and its interaction with the Si surface. The shift carbonyl stretching of urea (1624 cm–1) and broadening of the silanol O–H peak (3270 cm–1) indicate hydrogen bonding between urea’s amine groups and Si’s hydroxyl functionalities, providing direct spectroscopic evidence for the proposed dispersion mechanism.

The silane-treated formulation (IR-Si/Si-75) shows intensified absorption at 1082 cm–1, attributed to enhanced Si–O–Si stretching associated with siloxane bridge formation during silanization reactions. This spectroscopic evidence correlates directly with the improved mechanical properties and reduced Payne effect observed in silane-containing formulations, confirming the successful chemical coupling between the filler and matrix. The combined system (IR-Si/urea/Si-75) exhibits the most comprehensive spectral modifications, displaying characteristic features of both urea–Si interactions (peaks at 692–669 cm–1 and 1545, 1624 cm–1) and decreased absorption peaks appear at 3270 cm–1 (O–H stretching), which enhanced silanization (intensified Si–O–Si stretching). This spectroscopic synergy provides molecular-level validation of the dual-mechanism approach and explains why the combined system achieves superior performance compared to individual additives.

Based on the comprehensive characterization results, Figure illustrates the molecular mechanisms underlying the synergistic effects of urea and silane in Si-filled IR composites. These mechanisms directly explain the enhanced cure characteristics, improved dispersion, and superior mechanical properties observed in this study.

7.

7

Schematic representation of the coupling mechanisms in Si-filled IR composites: (a) IR-Si/Si-75, (b) IR-Si/urea, and (c) IR-Si/urea/silane.

The silane coupling mechanism (Figure a) involves the bifunctional nature of Si-75, which contains triethoxysilyl groups that undergo hydrolysis and condensation reactions with silanol groups on the Si surface, forming stable siloxane bridges (Si–O–Si). Simultaneously, the disulfide functionality reacts with rubber chains during vulcanization, creating covalent bonds between the filler and matrix. , This dual reactivity explains the enhanced cross-link density and mechanical properties observed in silane-treated formulations. The mechanism of urea in Si-filled IR composites can be explained by the interaction between the amine groups of urea and the hydroxyl (–OH) groups of silanol through hydrogen bonding (Figure b). This interaction enhances the dispersion of Si within the rubber matrix. The synergistic mechanism (Figure c) demonstrates how urea functions as a silanization catalyst when it is combined with Si-75. The amine functionalities of urea coordinate with silanol groups, activating them for condensation reactions with silane coupling agents. This catalytic effect accelerates siloxane bridge formation, leading to more efficient chemical coupling and explaining the superior performance of the combined system. The enhanced silanization efficiency directly correlates with the highest cross-link density, maximum mechanical properties, and finest morphological dispersion observed in the IR-Si/urea/Si-75 formulation.

3.7. Dynamic Mechanical Properties

Figure presents the temperature-dependent storage modulus and loss tangent (tan δ) profiles, demonstrating how enhanced network formation translates into superior dynamic performance.

8.

8

(a) Storage modulus and (b) tan delta (δ) of silica-filled polyisoprene rubber composites without and with different coupling agents.

The storage modulus behavior exhibits distinct temperature-dependent trends that validate the proposed reinforcement mechanisms. In the glassy region below T g , the IR-Si/urea formulation demonstrated the highest storage modulus, followed by IR-Si/Si-75/urea, IR-Si/Si-75, IR-Si, and neat IR vulcanizate (Figure a). This ranking reflects the restricted molecular mobility achieved through improved filler dispersion and enhanced filler–rubber interactions, consistent with the bound rubber and cross-link density findings discussed in Sections –3.3. During the glass transition and into the rubbery region, the storage modulus ranking shifted to IR-Si > IR-Si/urea > IR-Si/Si-75 > IR-Si/Si-75/urea > neat IR. This behavior indicates that while Si provides inherent stiffness through particle reinforcement, the chemical modifications alter the temperature sensitivity of the composite network. The reduced temperature dependence in treated formulations suggests more homogeneous stress distribution and improved thermal stability of the cross-linked network.

The glass transition temperatures, determined from tan δ peak positions (Figure b), are summarized in Table and provide important insights into the nature of filler–polymer interactions. The neat IR vulcanizate exhibited a T g of −43.96 °C, while the incorporation of Si alone (IR-Si) showed a nearly identical T g (−44.04 °C). The addition of urea (IR-Si/urea) and silane (IR-Si/Si-75) resulted in T g values of −43.42 and −43.24 °C, respectively, whereas the combination of both additives (IR-Si/Si-75/urea) yielded a T g of −43.71 °C. Importantly, all observed T g values fall within the typical experimental accuracy of DMA measurements, indicating that all formulations exhibit statistically similar glass transition temperatures. This finding suggests that urea and silane act primarily as compatibilizers that improve filler dispersion and interfacial adhesion, rather than inducing molecular-level miscibility that would significantly alter the polymer’s glass transition behavior. , The absence of substantial T g shifts, despite notable improvements in mechanical properties (as demonstrated by tensile testing), confirms that the reinforcement mechanisms operate mainly through interfacial modification, enhancing filler–rubber adhesion via hydrogen bonding at particle surfaces and improved stress transfer efficiency without fundamentally altering polymer chain mobility. This behavior is characteristic of well-dispersed composite systems, where reinforcement arises from morphological improvements, which were confirmed by SEM images.

5. Glass Transition Temperature (T g), Tan δ at 0 °C, and Tan δ at 60 °C of Silica-Filled Isoprene Rubber Composites.

  dynamic mechanical properties
samples T g (°C) tan δ at 0 °C tan δ at 60 °C
Neat IR vulcanizate –43.96 0.086 0.092
IR-Si –44.04 0.092 0.102
IR-Si/urea –43.42 0.181 0.182
IR-Si/Si-75 –43.24 0.013 0.022
IR-Si/Si-75/urea –43.71 0.124 0.122

The tan δ values at 0 and 60 °C reveal the critical trade-off between wet grip and rolling resistance. At 0 °C, high tan δ indicates a superior wet grip. The IR-Si/urea composite had the highest tan δ (0.181), suggesting an outstanding wet grip due to strong hydrogen bonding between urea and Si. Conversely, the IR-Si/Si-75 compound showed the lowest tan δ (0.013), indicating poor wet grip. At 60 °C, low tan δ is desirable for low rolling resistance and improved fuel efficiency. The IR-Si/Si-75/urea composite is a key finding in balancing these properties, which tan δ at 0 °C (0.124) is significantly higher than the silane-only system, demonstrating that urea effectively increased damping properties needed for good wet grip property. This synergy offers a promising strategy for optimizing the fuel efficiency-wet grip trade-off.

The maintained T g values across all formulations, combined with the significant mechanical property improvements, validate the proposed mechanism, where urea enhances filler–rubber compatibility through surface interactions and dispersion enhancement, creating a miscible blend system that preserves the fundamental thermal characteristics of the polyisoprene matrix while dramatically improving composite performance through optimized filler–polymer interfacial interactions. These findings provide definitive evidence that the dual-mechanism approach successfully optimizes the dynamic performance of Si-filled IR composites, translating the structural improvements into superior practical applications.

4. Conclusions

From the experimental results of this study, interesting conclusions can be drawn. Urea significantly improves the compatibility between Si and rubber by minimizing filler–filler interactions, leading to better dispersion of Si in the polyisoprene matrix. When combined with silane Si-75, urea promotes faster silanization and enhances Si surface modification. This combination also increases the cross-link density and bound rubber content, resulting in improved mechanical properties such as higher tensile strength and moduli at 100% and 300% elongation. These enhancements occur regardless of whether silane Si-75 is present. FTIR analysis confirmed the chemical interaction by hydrogen bonding between urea and Si as well as the silanization reaction. SEM observations demonstrated that urea reduces Si agglomerates and achieves a more uniform dispersion. DMA analysis revealed that urea and Si-75 enhanced storage modulus performance while maintaining similar glass transition temperatures, confirming their role as effective compatibilizers promoting improved filler dispersion and interfacial interactions. The reduced tan δ values at 0 and 60 °C indicate lower energy dissipation beneficial for tire traction, while the decreased Payne effect in urea-containing formulations demonstrates enhanced Si dispersion within the rubber matrix. Furthermore, urea’s nontoxic and biodegradable properties offer a sustainable solution for advancing tire performance and environmental safety in the rubber industry.

Acknowledgments

The author gratefully acknowledges the financial support from the Prince of Songkla University, Surat Thani Campus (Grant No. SIT6503039S) and the Faculty of Science and Industrial Technology for providing facilities and equipment. We are grateful to Assoc. Prof. Dr. Seppo Karrila for his assistance with manuscript preparation.

The authors declare no competing financial interest.

References

  1. Wu Q., Liu L., Meng J., Liu S., Hui J., Wang X., Xu L., Zhang L.. Microstructure and performance of green Tire tread based on epoxidized solution polymerized styrene butadiene rubber and epoxidized natural rubber. Ind. Eng. Chem. Res. 2023;62:5582–5593. doi: 10.1021/acs.iecr.3c00046. [DOI] [Google Scholar]
  2. Neethirajan J., Parathodika A. R., Hu G. H., Naskar K.. Functional Rubber Composites Based on Silica–Silane Reinforcement for Green Tire Application: The State of the Art. Funct. Compos. Mater. 2022;3:7. doi: 10.1186/s42252-022-00035-7. [DOI] [Google Scholar]
  3. Sarkawi S. S., Dierkes W. K., Noordermeer J. W.. Elucidation of Filler-to-Filler and Filler-to-Rubber Interactions in Silica-Reinforced Natural Rubber by TEM Network Visualization. Eur. Polym. J. 2014;54:118–127. doi: 10.1016/j.eurpolymj.2014.02.015. [DOI] [Google Scholar]
  4. Shahidizadeh A., Pircheraghi G., Shojaei M.. Reinforcing Performance of Silane-Modified Recycled Nanosilica within Sustainable, Non-black-filled Styrene–Butadiene Rubber Nanocomposites. ACS Sustainable Resource Management. 2024;1:857–867. doi: 10.1021/acssusresmgt.3c00083. [DOI] [Google Scholar]
  5. Braum M. V., Jacobi M. A.. Silica Grafted with Epoxidized Liquid Polybutadienes: Its Behavior as Filler for Tire Tread Compounds. Rubber Chem. Technol. 2017;90:173–194. doi: 10.5254/rct.16.83760. [DOI] [Google Scholar]
  6. Hussain M., Yasin S., Ali A., Li Z., Fan X., Song Y., Zheng Q., Wang W.. Synergistic Impact of Ionic Liquid on Interfacial Interaction and Viscoelastic Behaviors of Silica Filled Nitrile Butadiene Rubber Nanocomposites. Compos. Part A: Appl. Sci. Manuf. 2022;163:107202–107211. doi: 10.1016/j.compositesa.2022.107202. [DOI] [Google Scholar]
  7. Chi C., Wang P., Qian W., Zhang Y., Chen Q.. Cardanol grafted onto liquid isoprene rubber like ground brothers hanging on the vine: A green plasticizer and compatibilizer. Mater. Today Commun. 2022;32:104116. doi: 10.1016/j.mtcomm.2022.104116. [DOI] [Google Scholar]
  8. Wang X., Wu L., Yu H., Xiao T., Li H., Yang J.. Analysis of Effect of Modification of Silica and Carbon Black Co-Filled Rubber Composite on Mechanical Properties. e-Polym. 2021;21:279–288. doi: 10.1515/epoly-2021-0034. [DOI] [Google Scholar]
  9. Sarkawi, S. S. Silica-Reinforced Deproteinized Natural Rubber. In Silicon Materials; Intech Open: London, UK, 2019. [Google Scholar]
  10. Moretto E., Fernandes J. P., Staropoli M., Rogé V., Steiner P., Duez B., Lenoble D., Thomann J. S.. Dual-silane premodified silica nanoparticles– synthesis and interplay between chemical, mechanical, and curing properties of silica–rubber nanocomposites: application to tire tread compounds. ACS omega. 2022;7:17692–17702. doi: 10.1021/acsomega.2c00665. [DOI] [PMC free article] [PubMed] [Google Scholar]
  11. Azizi S., Momen G., Ouellet-Plamondon C., David E.. Performance improvement of EPDM and EPDM/Silicone rubber composites using modified fumed silica, titanium dioxide and graphene additives. Polym. Test. 2020;84:106281. doi: 10.1016/j.polymertesting.2019.106281. [DOI] [Google Scholar]
  12. Lockhorn D., Klüppel M.. Structure–Property Relationships of Silica/Silane Formulations in Natural Rubber, Isoprene Rubber, and Styrene–Butadiene Rubber Composites. J. Appl. Polym. Sci. 2020;137:48435. doi: 10.1002/app.48435. [DOI] [Google Scholar]
  13. Bignotti F., Borsacchi S., de Santis R., Geppi M., Messori M., Sudhakaran U. P.. Interrelation Between Preparation Conditions, Structure, and Mechanical Reinforcement in Isoprene Rubber Filled with In Situ Generated Silica. J. Appl. Polym. Sci. 2012;125:E398–E412. doi: 10.1002/app.36337. [DOI] [Google Scholar]
  14. Sun S., Tang F., Gong D.. Fabrication of cis-1,4 Polyisoprene Composites Reinforced with Well-Dispersed Silica/Carbon Black Promoted by Silica–Rubber Hydrogen-Bonding. Polym. Compos. 2025;46:6070–6082. doi: 10.1002/pc.29343. [DOI] [Google Scholar]
  15. Sarkawi S. S., Kaewsakul W., Sahakaro K., Dierkes W. K., Noordermeer J. W.. A review on reinforcement of natural rubber by silica fillers for use in low-rolling resistance tires. J. Rubber Res. 2015;18:203–233. [Google Scholar]
  16. Wang D., Tang Z., Huang R., Li H., Zhang C., Guo B.. Inverse vulcanization of vinyltriethoxysilane: A novel interfacial coupling agent for silica-filled rubber composites. Macromolecules. 2022;55:8485–8494. doi: 10.1021/acs.macromol.2c01678. [DOI] [Google Scholar]
  17. Yang L., Sun S., Yu X., Xu Z., Lu Y., Shi X., Song Y., Wang D., Zuo M., Zheng Q.. Effect of Deep Eutectic Solvents on Vulcanization Kinetics and Strain-Softening Behavior of Natural Rubber/Styrene-Butadiene Rubber. Polymer. 2025;316:127871. doi: 10.1016/j.polymer.2024.127871. [DOI] [Google Scholar]
  18. Wolff S., Wang M. J., Tan E. H.. Filler-Elastomer Interactions. Part VII. Study on Bound Rubber. Rubber Chem. Technol. 1993;66:163–177. doi: 10.5254/1.3538304. [DOI] [Google Scholar]
  19. Sattayanurak S., Sahakaro K., Kaewsakul W., Dierkes W. K., Reuvekamp L. A., Blume A., Noordermeer J. W.. Enhancing Performance of Silica-Reinforced Natural Rubber Tire Tread Compounds by Applying Organoclay as Secondary Filler. Rubber Chem. Technol. 2021;94:121–144. doi: 10.5254/rct.20.80373. [DOI] [Google Scholar]
  20. Ridho M. R., Agustiany E. A., Rahmi D. N. M., Madyaratri E. W., Ghozali M., Restu W. K., Falah F., Rahandi Lubis M. A., Syamani F. A., Nurhamiyah Y., Hidayati S.. Lignin as Green Filler in Polymer Composites: Development Methods, Characteristics, and Potential Applications. Adv. Mater. Sci. Eng. 2022:1363481. doi: 10.1155/2022/1363481. [DOI] [Google Scholar]
  21. Arroyo M., Lopez-Manchado M. A., Valentin J. L., Carretero J.. Morphology/Behavior Relationship of Nanocomposites Based on Natural Rubber/Epoxidized Natural Rubber Blends. Compos. Sci. Technol. 2007;67:1330–1339. doi: 10.1016/j.compscitech.2006.09.019. [DOI] [Google Scholar]
  22. Zhao M., Lv W., Li Y., Dai C., Wang X., Zhou H., Zou C., Gao M., Zhang Y., Wu Y.. Study on the Synergy between Silica Nanoparticles and Surfactants for Enhanced Oil Recovery during Spontaneous Imbibition. J. Mol. Liq. 2018;261:373–378. doi: 10.1016/j.molliq.2018.04.034. [DOI] [Google Scholar]
  23. Bornstein D., Pazur R. J.. The Sulfur Reversion Process in Natural Rubber in Terms of Crosslink Density and Crosslink Density Distribution. Polym. Test. 2020;88:106524. doi: 10.1016/j.polymertesting.2020.106524. [DOI] [Google Scholar]
  24. Han Y., Zheng H., Liu Y., Wang M., Wang J., Xie Q., Jing S., Qin X., Zhang L.. Synergistic development of natural rubber/butyl rubber composites for improved interfacial bonding and enhanced shock-absorbing capabilities. ACS omega. 2024;9:13897–13905. doi: 10.1021/acsomega.3c08996. [DOI] [PMC free article] [PubMed] [Google Scholar]
  25. Hayichelaeh C., Reuvekamp L. A. E. M., Blume A., Noordermeer J. W. M., Sahakaro K.. Reinforcement of Natural Rubber by Silica/Silane in Dependence of Different Amine Types. Rubber Chem. Technol. 2017;90:651–666. doi: 10.5254/rct.82.83708. [DOI] [Google Scholar]
  26. Zhong X., Song Y., Zheng Q.. Payne Effect and Mullins Effect of Silica Filled Butadiene Rubber Nanocomposites Vulcanizates and Their Unextractable Gels. Polymer. 2023;267:125634. doi: 10.1016/j.polymer.2022.125634. [DOI] [Google Scholar]
  27. Kandil H., Abo-Salem H. M.. A Novel Thiourea-Based Interfacial Modifier for Silica-Filled Natural Rubber Composites. J. Appl. Polym. Sci. 2023;140:e53550. doi: 10.1002/app.53550. [DOI] [Google Scholar]
  28. Huang L., Yu F., Liu Y., Lu A., Song Z., Liu W., Xiong Y., He H., Li S., Zhao X.. et al. Understanding the reinforcement effect of fumed silica on silicone rubber: bound rubber and its entanglement network. Macromolecules. 2022;56:323–334. doi: 10.1021/acs.macromol.2c01969. [DOI] [Google Scholar]
  29. Chino K.. Structure of Multinetwork Elastomer: Comparison with Hydrogen Bond Cross-Linking Elastomer. ACS omega. 2022;7:37520–37531. doi: 10.1021/acsomega.2c04296. [DOI] [PMC free article] [PubMed] [Google Scholar]
  30. Tanabe Y., Miyoshi K., Kirino Y.. Effect of Lewis Acid/Base Adducts as a Silanization Catalyst in Rubber Compositions Containing Silica. Rubber Chem. Technol. 2016;89:349–357. doi: 10.5254/rct.16.84836. [DOI] [Google Scholar]
  31. Wang X., Wu L., Yu H., Xiao T., Li H., Yang J.. Modified Silica-Based Isoprene Rubber Composite by a Multi-Functional Silane: Preparation and Its Mechanical and Dynamic Mechanical Properties. Polym. Test. 2020;91:106840. doi: 10.1016/j.polymertesting.2020.106840. [DOI] [Google Scholar]
  32. Ahn B., Kim D., Kim K., Kim I. J., Kim H. J., Kang C. H., Lee J. Y., Kim W.. Effect of the Functional Group of Silanes on the Modification of Silica Surface and the Physical Properties of Solution Styrene-Butadiene Rubber/Silica Composites. Compos. Interfaces. 2019;26:585–596. doi: 10.1080/09276440.2018.1514145. [DOI] [Google Scholar]
  33. Sun Y., Cheng Z., Zhang L., Jiang H., Li C.. Promoting the Dispersibility of Silica and Interfacial Strength of Rubber/Silica Composites Prepared by Latex Compounding. J. Appl. Polym. Sci. 2020;137:49526. doi: 10.1002/app.49526. [DOI] [Google Scholar]
  34. Yan H., Sun K., Zhang Y., Zhang Y.. Effect of Nitrile Rubber on Properties of Silica-Filled Natural Rubber Compounds. Polym. Test. 2005;24:32–38. doi: 10.1016/j.polymertesting.2004.07.011. [DOI] [Google Scholar]
  35. Bera A., Ganguly D., Rath J. P., Ramakrishnan S., Kuriakose J., Amarnath S. K. P., Chattopadhyay S.. The Effect of Bio-Based Ingredients in Isoprene Rubber: A Biomimetic Approach to Improve the Dispersion of Silica. Mater. Chem. Phys. 2023;295:127151. doi: 10.1016/j.matchemphys.2022.127151. [DOI] [Google Scholar]
  36. Nguyen C. H., Fu C. C., Chen Z. H., Tran T. T. V., Liu S. H., Juang R. S.. Enhanced and Selective Adsorption of Urea and Creatinine on Amine-Functionalized Mesoporous Silica SBA-15 via Hydrogen Bonding. Mesoporous Mater. 2021;311:110733. doi: 10.1016/j.micromeso.2020.110733. [DOI] [Google Scholar]
  37. Lee S. Y., Kim J. S., Lim S. H., Jang S. H., Kim D. H., Park N. H., Jung J. W., Choi J.. The Investigation of the Silica-Reinforced Rubber Polymers with the Methoxy Type Silane Coupling Agents. Polymers. 2020;12:3058. doi: 10.3390/polym12123058. [DOI] [PMC free article] [PubMed] [Google Scholar]
  38. Wei L., Shen M., Xin Z.. A Novel Material Based on Deep Eutectic Solvents and Its Application in In-Situ Modified Silica-Reinforced Styrene-Butadiene Rubber. J. Appl. Polym. Sci. 2022;139:52089. doi: 10.1002/app.52089. [DOI] [Google Scholar]
  39. Hayichelaeh C., Reuvekamp L. A. E. M., Dierkes W. K., Blume A., Noordermeer J. W. M., Sahakaro K.. Enhancing the Silanization Reaction of the Silica-Silane System by Different Amines in Model and Practical Silica-Filled Natural Rubber Compounds. Polymers. 2018;10:584. doi: 10.3390/polym10060584. [DOI] [PMC free article] [PubMed] [Google Scholar]
  40. Esmaeeli R., Tada T., Farhad S.. A New High Frequency Dynamic Mechanical Analysis System: An Approach to Direct High Frequency Testing of Tire Tread Rubber. Polym. Test. 2020;86:106491. doi: 10.1016/j.polymertesting.2020.106491. [DOI] [Google Scholar]
  41. Nuinu P., Sirisinha C., Suchiva K., Daniel P., Phinyocheep P.. Improvement of Mechanical and Dynamic Properties of High Silica Filled Epoxide Functionalized Natural Rubber. J. Mater. Res. Technol. 2023;24:2155–2168. doi: 10.1016/j.jmrt.2023.03.101. [DOI] [Google Scholar]
  42. Aini N. A. M., Othman N., Hussin M. H., Sahakaro K., Hayeemasae N.. Efficiency of Interaction between Hybrid Fillers Carbon Black/Lignin with Various Rubber-Based Compatibilizer, Epoxidized Natural Rubber, and Liquid Butadiene Rubber in NR/BR Composites: Mechanical, Flexibility and Dynamical Properties. Ind. Crops Prod. 2022;185:115167. doi: 10.1016/j.indcrop.2022.115167. [DOI] [Google Scholar]

Articles from ACS Omega are provided here courtesy of American Chemical Society