Abstract
Objectives
This study evaluated the mechanical and surface characteristics of the transition zone of multilayered translucent zirconia (TZ) after aging and analyzed the correlation between the 4-point bending flexural strength (4PBFS) and biaxial flexural strength (BFS) in each zone.
Methods
Traditional (3Y-TZP of LT; L, 4Y-TZP of MT; M) and multilayered TZ (5Y-TZP of MT Multi; T, 3Y/5Y-TZP of Prime; P, 4Y/5Y-TZP of Prime esthetic; E) IPS E.max ZirCAD blocks were used to fabricate 525 disk-shaped and 300 bar-shaped specimens. Specimens were separated into three groups, aged in an autoclave at 134 °C under 0.2 MPa for 0 h, 5 h, and 10 h. The mechanical and surface characteristics of the transition zone in multilayered TZ were analyzed, following statistical analyses (α = 0.05).
Results
L showed the highest 4PBFS and BFS, irrespective of aging. Consistent correlations between the 4PBFS and BFS were found in all groups. L showed the highest Weibull characteristic strength under all conditions. T showed the highest nanoindentation hardness and Young’s modulus, and the Vickers hardness of L and P were lower than other groups. Aging led to surface uplifts and microcracks caused by phase transformation, particularly in L and P.
Conclusions
The flexural strength of 3Y/5Y-TZP and 4Y/5Y-TZP was comparable to that of 3Y-TZP and 4Y, 5Y-TZP respectively, regardless of aging. Surface roughness showed a marked increase after aging in 3Y-TZP and 3Y/5Y-TZP. Furthermore, the interaction between yttria content and aging was evident across all mechanical and surface characteristics, except for flexural strength.
Graphical Abstract

Introduction
The primary goal in the development of dental ceramics is to manufacture materials with excellent aesthetics and sufficient strength for long-term durability. Zirconia can exist in three different crystallographic forms determined by the temperature and pressure: cubic (c) at temperatures >2370 °C, tetragonal (t) at temperatures >1170 °C, and monoclinic (m) at room temperature (21–23 °C) [1]. In zirconia, phase transformation from tetragonal to monoclinic (t → m) results in a 4% volumetric increase [2]. Under loading conditions, the controlled expansion of zirconia can hinder microcrack progression, increasing its toughness through a process called transformation toughening [3]. Adding stabilizing oxides such as yttria (Y2O3) to pure zirconia allows tetragonal phase retention at room temperature (21–23 °C) and enables controlled t → m transformation, leading to high fracture toughness [4].
Zirconia-based materials (such as 3Y-TZP; 3 mol% yttria-stabilized tetragonal zirconia polycrystals) were first applied in dentistry after tetragonal-form stabilization with yttria (3 mol%) owing to their outstanding mechanical properties resulting from the toughening mechanism of stress-induced phase transformation [5, 6]. However, poor translucency, primarily due to the large birefringence effect of tetragonal phase zirconia, limited their applicability to posterior restorations [3, 7]. Therefore, low-opacity Zirconia-based materials stabilized with high yttria contents were subsequently manufactured [1]. With the advent of 4Y-PSZ (4 mol% yttria-partially stabilized zirconia, 25% cubic phase) and 5Y-PSZ (5 mol% yttria-partially stabilized zirconia, 50% cubic phase), zirconia crystals were stabilized in the non-birefringent cubic and tetragonal forms, resulting in high translucency and good aesthetics [8]. However, the improvement in translucency is accompanied with a reduction in flexural strength and toughness owing to the high stability of the cubic lattice and relatively poor ability of stress-induced transformation toughening [9]. Thus, zirconia with higher translucency showed lower strength [10].
Recently developed multilayered zirconia blocks enable the production of zirconia restorations with both translucency (for a natural appearance) and acceptable mechanical properties [11]. Shade-gradient multilayered zirconia contains layers of varying shades along with a single yttria content and phase composition; in contrast, strength-gradient zirconia comprises polychromatic multilayer zirconia with a hybrid yttria content and phase composition [12, 13]. A typical strength-gradient multilayer zirconia block is composed of a highly translucent enamel layer of 5Y-TZP, a transition layer of 3Y-TZP/5Y-TZP or 4Y-TZP/5Y-TZP, and a body layer of 3Y-TZP or 4Y-TZP for mechanical strength [14–16].
In this study, two different multilayered translucent zirconia (TZ) systems: IPS E.max ZirCAD Prime and IPS E.max ZirCAD Prime esthetic (Ivoclar Vivadent Inc., Schaan, Lichtenstein), with transition zone compositions of 3Y/5Y-TZP and 4Y/5Y-TZP, respectively, were used. The transition zone refers to the middle compositional layer in multilayered TZ blocks that is designed to achieve a smooth gradient in both chroma and yttria concentration from the dentin (3Y-TZP or 4Y-TZP) to the incisal (5Y-TZP) region.
The layered manufacturing technique used to produce multilayered TZ blanks is reported to result in prostheses with poor mechanical properties owing to weak interfaces [17]. As multilayered computer-aided design/computer-aided manufacturing (CAD/CAM) blanks are manufactured by a pressing technique in which various zirconia powders are pressed to form a single metal mold, they are susceptible to interfacial flaws, including impurities and partially sintered particles [18, 19]. Therefore, several studies have studied the mechanical and surface characteristics of the transition zone of strength-gradient multilayered TZ [12, 15, 20–22].
Because dental ceramics are highly brittle, flexural strength is a critical parameter for evaluating their mechanical properties [23]. The distribution and presence of internal defects, which influence the strength of dental ceramics, are evaluated using the Weibull modulus, which describes the variability in the measured strengths of brittle materials [24]. ISO 6872:2015, which defines standardized testing methods for dental ceramics, proposes the 4-point bend test, 3-point bend test, and piston-on-3 ball test (i.e., the biaxial flexural strength (BFS) test) as standardized methods for evaluating the flexural strength of zirconia [25]. However, few studies on the mechanical properties of multilayered TZ have probed into the correlation between the results and reliability of these flexural strength testing methods.
To evaluate the prognosis of Y-TZP prostheses in the oral cavity, considering the effect of LTD (low-temperature degradation) from hydrothermal aging is critical [26–30]. In clinical situations, Y-TZP restorations encounter challenges such as humidity, changes in pH, cyclic loading from mastication, and low temperatures for t-phase stabilization [31]. Aging occurs from gradual t → m transformation on Y-TZP exposed to water or body fluid, at a wide temperature range (37–500 °C) [31–33]. This transformation, influenced by grain size, yttria content, grain alignment, residual surface stress, and proportion of cubic phase, induces rough surfaces and pull-out of grains [34, 35]. A 4% volume increase in one grain that transforms into the monoclinic phase induces compressive stresses in the adjacent grains, which induce additional phase transformation and microcrack propagation; this facilitates water infiltration, compromising the mechanical properties of the system [31, 36]. Because aging is activated by thermal conditions, aging tests can be accelerated by pressure and temperatures higher than body temperature (37 °C), such as temperature in an autoclave (134 °C). In 1999, Chevalier et al. suggested that 1 h of hydrothermal aging in an autoclave is equal to 3–4 years in vivo [26]. Several studies have explored the influence of hydrothermal aging on the mechanical and surface characteristics of TZ with different concentrations of yttria [37–40]. However, few studies have evaluated the effects of hydrothermal aging on the mechanical and surface characteristics of the different layers of strength-gradient multilayer zirconia.
Thus, the purpose of this study was to probe into the differences in the mechanical and surface characteristics of different zones in traditional and multilayered TZ containing varying amounts of yttria. The 4PBFS and BFS of the transition zone of multilayered TZ samples were compared to determine the correlation between these two types of flexural strength and to identify the flexural strength with higher reliability for representing the mechanical properties of zirconia. The following four null hypotheses were used in this study: i) no significant variation exists in the mechanical and surface characteristics across different compositional zones—including the transition zone—before and after hydrothermal aging; ii) the gradient distribution of yttria content across multilayered zirconia does not significantly influence the mechanical and surface characteristics; iii) the mechanical and surface characteristics of gradient zones in TZ after hydrothermal aging are not influenced by their yttria content; and iv) no correlation exists between the 4PBFS and BFS of zones consisted of various mounts of yttria.
Materials and Methods
Specimen preparation
In this study, five different TZ systems (IPS E.max ZirCAD; Ivoclar Vivadent Inc., Schaan, Lichtenstein) were used for experimentation; two types of traditional TZ blocks (IPS E.max ZirCAD LT, L; IPS E.max ZirCAD MT, M) and three types of multilayered TZ blocks (IPS E.max ZirCAD MT Multi, T; IPS E.max ZirCAD Prime, P; IPS E.max ZirCAD Prime Esthetic, E) were investigated (Table 1).
Table 1.
Composition and other details of the tested materials provided by the manufacturers
| Material | Manufacturer | Composition | Shade (Size) | Lot number |
|---|---|---|---|---|
| IPS E.max ZirCAD LT | Ivoclar Vivadent |
3Y-TZP Zirconium oxide (88.0–95.5 wt%) Yttrium oxide (4.5–6.0 wt%) Hafnium oxide (≤5.0 wt%) Aluminium oxide (≤1.0 wt%) Other oxides (≤1.0 wt%) |
2 (Ø98.5 × 18.0 mm) | Z02R0D |
| IPS E.max ZirCAD MT | Ivoclar Vivadent |
4Y-TZP Zirconium oxide (86.0–93.5 wt%) Yttrium oxide (6.5–8.0 wt%) Hafnium oxide (≤5.0 wt%) Aluminium oxide (≤1.0 wt%) Other oxides (≤1.0 wt%) |
A2 (Ø98.5 × 18.0 mm) |
Z01WN7 Z02BMV |
| IPS E.max ZirCAD MT Multi | Ivoclar Vivadent |
4Y-TZP / 5Y-TZP Zirconium oxide (86.0–93.5 wt%) Yttrium oxide (6.5–8.0 wt%) Hafnium oxide (≤5.0 wt%) Aluminium oxide (≤1.0 wt%) Other oxides (≤1.0 wt%) |
A2 (Ø98.5 × 20.0 mm) |
Z02TJS Z031ST |
| IPS E.max ZirCAD Prime | Ivoclar Vivadent |
3Y-TZP / 5Y-TZP Zirconium oxide (88.0–95.5 wt%) Yttrium oxide (4.5–7.0 wt%) Hafnium oxide (≤5.0 wt%) Aluminium oxide (≤1.0 wt%) Other oxides (≤1.5 wt%) |
A2 (Ø98.5 × 25.0 mm) | Z03FTB |
| IPS E.max ZirCAD Prime esthetic | Ivoclar Vivadent |
4Y-TZP / 5Y-TZP Zirconium oxide (88.0–95.5 wt%) Yttrium oxide (4.5–7.0 wt%) Hafnium oxide (≤5.0 wt%) Aluminium oxide (≤1.0 wt%) Other oxides (≤1.5 wt%) |
A2 (Ø98.5 × 25.0 mm) | YB72LF |
825 specimens were separated into 5 groups (n = 165) for assessment of mechanical and surface characteristics. In each group, 105 specimens were designed in the form of disks for BFS and surface characteristics analyses, whereas the remaining 60 specimens were designed in the form of bars for 4PBFS tests. Considering a shrinkage rate of 20%, standardized disk-shaped zirconia specimens (diameter: 18.2 mm, thickness: 3.0 mm) and bar-shaped specimens (length: 55.0 mm, width: 5.0 mm, thickness: 4.0 mm) were designed using the CAD program (Solidworks, Dassault Systèmes, Paris, France) and manufactured using a precision milling machine (Cameleon CS, Neobiotech Co., Seoul, Republic of Korea). The incisal zone (5Y-TZP) was used to fabricate T specimens whereas the transition zones with an yttria composition of 3Y/5Y-TZP and 4Y/5Y-TZP, were used for P and E specimens respectively (Fig. 1). The specimens were sintered at 1500 °C, following the instructions provided by the manufacturer.
Fig. 1.

Design of specimens within multilayered blocks using CAD program. a T, b P, and c E. T, 5Y-TZP of IPS E.max ZirCAD MT Multi; P, 3Y/5Y-TZP of IPS E.max ZirCAD Prime; E, 4Y/5Y-TZP of IPS E.max ZirCAD Prime esthetic
Disk-shaped specimens, 1.2 mm thick and 15.0 mm in diameter were used for BFS testing, whereas bar specimens with a length of 45.0 mm, width of 4.0 mm, and thickness of 3.0 mm were used for 4PBFS testing. The four corners of the bar-shaped specimens were chamfered at 0.1 mm and 45°. Both the disk- and bar-shaped specimens were polished on the upper and bottom sides (the side with a diameter of 15.0 mm in the disk-shaped specimens, and the surface with a length of 45.0 mm and width of 4.0 mm in the bar-shaped specimens) using a grinding machine and 6-μm diamond slurry followed by 1-μm grit, in accordance with ISO 6872:2015 [25]
After grinding and polishing, a digital caliper was used to measure the size of each specimen. Subsequently, the specimens were heat treated in a furnace for 1 h within the temperature range of 900–1000 °C to induce a reverse phase transformation involving the conversion of monoclinic zirconia to tetragonal zirconia. All specimens were subjected to ultrasonic cleaning with distilled water and dried at room temperature (21–23 °C) for 24 h.
Hydrothermal aging process and selection of specimens
Each sample group was divided into three subgroups comprising 35 randomly selected disk-shaped and 20 bar-shaped specimens. The first subgroup was submerged in distilled water at room temperature (21–23 °C) for 24 h, dried for 24 h, and set as the control group. The second subgroup was aged in an autoclave (Hiclave H480S, Hongik Medical Systems) containing distilled water at 134 °C under 0.2 MPa for 5 h and used as first-aged group. The last subgroup was aged in an autoclave at 134 °C under 0.2 MPa for 10 h and used as second-aged group. (Table 2).
Table 2.
Abbreviations of the groups of tested materials
| Zone of material (Yttrium oxide content) | Material code | Groups | ||
|---|---|---|---|---|
| Control | First aged | Second aged | ||
| 3Y-TZP of IPS E.max ZirCAD LT | L | LC | LAF | LAS |
| 4Y-TZP of IPS E.max ZirCAD MT | M | MC | MAF | MAS |
| 5Y-TZP of IPS E.max ZirCAD MT Multi | T | TC | TAF | TAS |
| 3Y/5Y-TZP of IPS E.max ZirCAD Prime | P | PC | PAF | PAS |
| 4Y/5Y-TZP of IPS E.max ZirCAD Prime esthetic | E | EC | EAF | EAS |
Y-TZP Yttria-stabilized tetragonal zirconia polycrystal
Twenty bar-shaped specimens from each subgroup (i.e., from the control, first-aged, and second-aged subgroups) were used for 4PBFS testing. The mechanical properties of 20 of the 35 disk-shaped specimens were used for BFS testing. The remaining 15 disk-shaped specimens were used for surface characteristics analysis and Vickers hardness tests. Among these 15 specimens, one was randomly selected for X-ray diffraction (XRD). Nine additional specimens were used for nanoindentation hardness and Young’s modulus tests; atomic force microscopy (AFM) and confocal laser scanning microscopy (CLSM) were performed sequentially on the same side of each of these nine specimens. Three measurements were recorded for each specimen (i.e., a total of 27 measurements) during nanoindentation hardness and Young’s modulus analyses, AFM, and CLSM. The other side of these nine specimens, the sample used for XRD, and the remaining five unused specimens (i.e., a total of 15 disk-shaped specimens) were subjected to Vickers hardness testing. The Vickers hardness was measured thrice per specimen (i.e., a total of 45 measurements were recorded). Finally, the side not subjected to the Vickers hardness test in the five previously mentioned specimens (which were not subjected to nanoindentation hardness and Young’s modulus tests, AFM, and CLSM) was used for field emission scanning electron microscopy (FE-SEM) and energy dispersive X-ray spectroscopy (EDS).
Comparative analysis of mechanical properties
Twenty bar-shaped specimens were used for 4PBFS testing following ISO 6872:2015 guidelines [25] by a universal testing machine (Instron 5583, Instron Co., Norwood, MA, USA) with a 5-kN load cell at a crosshead speed of 0.5 mm/min. The bar-shaped specimens were located at the center of four support rollers with a diameter of 3 mm. The distance between the outer and inner rollers was 40 and 20 mm, respectively. The load was increased until the specimens fractured; maximum fracture load (P) of each specimen was recorded in N, and flexural strength (σ) was determined in MPa using the equation below:
| 1 |
where b is the height of the specimen (mm), w is the width of the specimen (mm), and L is the distance between the outer support rollers (mm).
The BFS of 20 disk-shaped specimens was evaluated through tests stipulated by ISO 6872:2015 [25] using a universal testing machine (Instron 5583) with a 5-kN load cell. The test jig consisted of three steel balls with a diameter of 3 mm positioned at an angle of 120° to each other; the center of the jig, which functioned as a support circle for the specimen, was 11 mm in diameter. Each disk-shaped specimen was placed at the center of the three balls and loaded using a flat pin with a diameter of 1.5 mm and length of 2 mm at the crosshead speed of 0.5 mm/min. The load was increased until the specimen fractured; the maximum fracture load (P) of each specimen was recorded in N, and the flexural strength (σ) was calculated in MPa using the equations below:
| 2 |
| 3 |
| 4 |
where b is the height of the specimen (mm), v is the Poisson’s ratio (v = 0.3), r1 is the support circle radius (mm), r2 is the flat pin radius (mm), and r3 is the specimen radius (mm).
To evaluate the reliability of the specimens, two-parameter Weibull analysis was conducted. the Weibull modulus (w) and characteristic strength (σ0) were determined using Excel (Microsoft Inc) from the 4PBFS and BFS according to ISO 6872:2015 [25]. The σ values were aligned in ascending order and applied to the following equation:
| 5 |
where Pf is a fracture probability between 0 and 1, N is the number of specimens in the subgroup, and i represents the flexural strengths in ascending order. The sorted data were used to create a graph with ln σ on the x-axis and ln [1/(1 – Pf)] on y-axis. The slope and x-intercept of the graph indicated w and σ0, respectively.
The nanoindentation hardness and Young’s modulus of the disk-shaped specimens were tested with a 40-nm Berkovich diamond indenter with a nanoindenter using a maximum penetration depth of 2 µm and an essential load of 45 mN. The Poisson’s ratio was 0.3 [41]. An analysis software (TestWork Software, MTS Systems Co., Eden Prairie, MN, USA) was used for evaluation of the results.
Vickers hardness test was conducted on the specimens using a microhardness tester. Specimens were indented at three sites with a loading mass of 0.1 kgf (0.98 N) on each specimen [42]. The diagonal lengths of these indentations (mm) were calculated using an analysis software (AVPAK System B, Mitutoyo). The microhardness of the samples was estimated by the following equation:
| 6 |
where Hv is the Vickers hardness value at an applied force of F (kgf) and d is the mean length of the indentation diagonal (mm).
Comparative analysis of surface properties
The surface roughness (Ra and Rq,) of each disk-shaped specimen was measured thrice using CLSM. The specimens were magnified (20×) using a 543-nm helium–neon laser (1 mW). The measured area was 300 × 300 µm2, and an image examiner was used to ensure CLSM images with adequate resolution.
AFM was used to analyze the surface topography (Ra, Rq, Sa, and Sq) of the samples. Using AFM (XE-100, Park System, Suwon, Republic of Korea) in the non-contact mode, the surface roughness was measured thrice per specimen at a scan rate of 0.8 Hz. The data and scan sizes were 256 × 256 pixels and 10 × 10 μm2, respectively.
One specimen was selected from each subgroup, and XRD was conducted for crystalline phase analysis. XRD data were collected through the Bragg–Brentano geometry in the 2θ range of 24°–36° with Kα radiation on an XRD instrument. The following conditions were used for scanning: 30 mA, 40 kV, scanning rate of 0.25°/min, scan time of 8 s/step, and step size of 0.005°. The monoclinic phase peak intensity ratio (Xm) was calculated using the following equation [43]:
| 7 |
where Im and It indicate the integrated intensities of the monoclinic (111), ( and tetragonal (111) peaks, respectively, at 31°, 28°, and 30°. According to Toraya et al., the following equation can be used to calculate the monoclinic phase volume fraction (Fm), which is the percentage of tetragonal-to-monoclinic transformation in zirconia [44]:
| 8 |
FE-SEM was used to analyze the surface microstructures of the samples. The specimens were sputter-coated with platinum using a sputter coater at 20 mA for 15 s and observed at 30000× magnification under a measured voltage of 5.0 kV with an FE-SEM instrument.
EDS was used to investigate alterations in the elemental composition of the samples (Zr, O, Y, Al, and Hf) during aging under an accelerating voltage of 15.0 kV and 200× magnification.
Statistical analyses
Statistical analyses were performed using statistical software (SPSS Statistics for Windows v23.0, IBM Corp., Armonk, NY, USA). The Shapiro–Wilk test was used to assess normality; the data were normally distributed. Pearson’s correlation test was used to identify any correlation between the 4PBFS and BFS in each subgroup. One-way ANOVA was used for comparison of the mechanical and surface properties of each material and Tukey’s HSD test was used for post hoc analysis (α = 0.05). An independent samples t-test was conducted for analysis of variables associated with the mechanical and surface characteristics of the specimens before and after hydrothermal aging. Two-way ANOVA and Tukey’s HSD tests were used to investigate the interaction between material types with varying concentrations of yttria and aging (α = 0.05).
Results
The 4PBFS for all sample groups are shown in Fig. 2 and listed in Supplementary Table 1. The 4PBFS of P are similar to those of L and significantly higher than those of M, T, and E under all aging conditions (P < 0.05). The 4PBFS of E are similar to those of M and T under all aging conditions. The independent samples t-test results indicate negligible differences between the control and aged sub-groups in all five specimen groups.
Fig. 2.

Mean ± standard deviation values and statistical analysis of the 4-point bending flexural strength. L, 3Y-TZP of IPS E.max ZirCAD LT; M, 4Y-TZP of IPS E.max ZirCAD MT; T, 5Y-TZP of IPS E.max ZirCAD MT Multi; P, 3Y/5Y-TZP of IPS E.max ZirCAD Prime; E, 4Y/5Y-TZP of IPS E.max ZirCAD Prime esthetic. All data are presented as mean ± standard deviation values. *denotes a significant difference at P < 0.05
The Weibull analysis results for the 4PBFS are shown in Fig. 3. The Weibull moduli and characteristic strengths of all the groups are listed in Supplementary Table 2. In the control group, the Weibull modulus was the largest in M, followed by T, L, and E (in descending order), and smallest in P. T exhibited the highest value after first aging, followed by M, L, P, and E. After second aging, L exhibited the highest value, whereas E exhibited the lowest value. Before aging, the characteristic strength was the highest in L to T through P and M. Following first and second aging, L and T showed the highest and lowest values, respectively.
Fig. 3.
Probability plot for the Weibull analysis of the 4-point bending flexural strength for all specimen groups. L, 3Y-TZP of IPS E.max ZirCAD LT; M, 4Y-TZP of IPS E.max ZirCAD MT; T, 5Y-TZP of IPS E.max ZirCAD MT Multi; P, 3Y/5Y-TZP of IPS E.max ZirCAD Prime; E, 4Y/5Y-TZP of IPS E.max ZirCAD Prime esthetic
The BFS values of all groups are shown in Fig. 4 and listed in Supplementary Table 3. In the control and first-aged groups, the BFS values of P are higher than those of M, T, and E and lower than those of L. In the second-aged group, the BFS values of P are higher than those of T, similar to those of M and E, and lower than those of L. The BFS values of E were comparable to those of M and T, but lower than those of L and P in the control and first-aged groups. In the second-aged group, the BFS values of E were lower than those of L and similar to those of M, T, and P. Independent samples t-tests indicate negligible differences between the control and aged sub-groups in all five groups.
Fig. 4.

Mean ± standard deviation values and statistical analysis of the biaxial flexural strength. L, 3Y-TZP of IPS E.max ZirCAD LT; M, 4Y-TZP of IPS E.max ZirCAD MT; T, 5Y-TZP of IPS E.max ZirCAD MT Multi; P, 3Y/5Y-TZP of IPS E.max ZirCAD Prime; E, 4Y/5Y-TZP of IPS E.max ZirCAD Prime esthetic. All data are presented as mean ± standard deviation values. *denotes a significant difference at P < 0.05
The Weibull analysis results for the BFS of specimens in all groups are shown in Fig. 5. The Weibull moduli and characteristic strengths of all the groups are listed in Supplementary Table 4. In the control and first-aged groups, the Weibull modulus decreased in the following order: L > M > P > T > E. After second aging, L and E showed the highest and lowest Weibull moduli, respectively. Prior to aging, the characteristic strength decreased in the following order: L > P > E > T > M. Among the first-aged groups, L and M showed the highest and lowest characteristic strength value, respectively, and after second aging, L and T showed the highest and lowest characteristic strength value, respectively.
Fig. 5.
Probability plot for the Weibull analysis of the biaxial flexural strength for all the groups. L, 3Y-TZP of IPS E.max ZirCAD LT; M, 4Y-TZP of IPS E.max ZirCAD MT; T, 5Y-TZP of IPS E.max ZirCAD MT Multi; P, 3Y/5Y-TZP of IPS E.max ZirCAD Prime; E, 4Y/5Y-TZP of IPS E.max ZirCAD Prime esthetic
Pearson’s correlation analysis was used to evaluate the relevance of the 4PBFS and BFS values in each group. The correlation coefficients and coefficients of determination are shown in Fig. 6 and listed in Supplementary Table 5. In the control group, the coefficient of correlation (r) was the closest to 1.00 in L and T, and decreased in the following order: E > M > P. After first aging, L and T exhibited the strongest correlations, followed by P, M, and E. After second aging, P and E showed the strongest and weakest correlations, respectively. In L, T, and E, the control group showed the strongest correlation, which decreased with aging. Conversely, M and P showed enhanced correlation with aging. Before aging, the coefficient of determination decreased in the following order: T > L > E > M. Among the first-aged groups, T and E exhibited the highest and lowest r values, respectively, and among the second-aged groups, P and E showed the highest and lowest r values, respectively.
Fig. 6.
Pearson’s correlation analysis of the 4-point bending flexural strength and biaxial flexural strength for all specimen groups. L, 3Y-TZP of IPS E.max ZirCAD LT; M, 4Y-TZP of IPS E.max ZirCAD MT; T, 5Y-TZP of IPS E.max ZirCAD MT Multi; P, 3Y/5Y-TZP of IPS E.max ZirCAD Prime; E, 4Y/5Y-TZP of IPS E.max ZirCAD Prime esthetic
The nanoindentation hardness values are shown in Fig. 7a and listed in Supplementary Table 6A. In the control group, P showed values similar to those of L and E, which were higher than those of M and T. Following first aging, P and L showed similar nanoindentation hardness values, which are lower than those of M, T, and E. In the second-aged group, P showed nanoindentation hardness values that were lower than those of M, T, and E and higher than those of L. Among the control groups, E showed nanoindentation hardness values similar to those of L, M, T, and P. In the first- and second-aged groups, E showed values similar to those of M and T and higher than those of L and P. Independent samples t-test results revealed significant differences among the following subgroups of L: LC and LAF, LC and LAS, and LAF and LAS (P < 0.05). In M, a significant difference existed between the MC and MAS groups (P < 0.05). In P, a significant difference existed between the PC and PAF groups, and PC and PAS groups (P < 0.05). No significant differences were observed between the nanoindentation hardness values of T and E before and after aging.
Fig. 7.

Mean ± standard deviation values and statistical analysis. a nanoindentation hardness, b Young’s modulus, and c Vickers hardness. L, 3Y-TZP of IPS E.max ZirCAD LT; M, 4Y-TZP of IPS E.max ZirCAD MT; T, 5Y-TZP of IPS E.max ZirCAD MT Multi; P, 3Y/5Y-TZP of IPS E.max ZirCAD Prime; E, 4Y/5Y-TZP of IPS E.max ZirCAD Prime esthetic. All data are presented as mean ± standard deviation values. *denotes a significant difference at P < 0.05
The Young’s moduli of all groups are shown in Fig. 7b and listed in Supplementary Table 6B. In the control group, P showed Young’s modulus values similar to those of L and E, which were lower than those of M and T. After first aging, P showed Young’s modulus values similar to those of L and lower than those of M, T, and E. Among the second-aged groups, P showed Young’s modulus values lower than those of M, T, and E and higher than those of L. Among the control groups, E showed values similar to those of L and P and lower than those of M and T. After first aging, E showed Young’s modulus values lower than those of M and T and higher than those of L and P. In the second-aged groups, the Young’s modulus values of E were comparable to those of M, lower than those of T, and higher than those of L and P. Independent samples t-test results exhibited a significant difference between the Young’s moduli of LC and LAF, LC and LAS, and LAF and LAS (P < 0.05) in L. In M, a significant difference existed between the Young’s moduli of MC and MAS, as well as MAF and MAS (P < 0.05). In T, a significant difference existed between the Young’s moduli of TC and TAS (P < 0.05). In P, a significant difference existsed between the PC and PAF groups, and PC and PAS groups (P < 0.05). No significant differences were observed between the Young’s moduli of groups with different aging times in E.
The Hv values of all groups are shown in Fig. 7c and listed in Supplementary Table 7. Before and after aging, the values of P were higher than those of L and lower than those of M, T, and E. In the control groups, the values of E are similar to those of T, which were higher than those of L, M, and P. After first and second aging, the values of E were similar to those of M and T and higher than those of L and P. Independent samples t-test results indicated significant differences between the Hv values of the control and first-aged groups, control and second-aged groups, and first- and second-aged groups (P < 0.05) in all five materials (except M). In M, a significant difference was found between the Hv values of MC and MAF as well as those of MC and MAS (P < 0.05).
The two-way ANOVA results for each tested mechanical property are presented in Supplementary Table 8. No significant interactions were observed between the yttria content of the different zones and the aging time for 4PBFS and BFS (P > 0.05). Conversely, for the nanoindentation hardness, Young’s modulus, and Vickers hardness, significant interactions existed between the yttria content of different zones and the aging time (P < 0.05).
Representative CLSM images of all five groups are shown in Fig. 8a. Supplementary Table 9 summarizes the mean values, standard deviations, and statistical analyses results for surface roughness (Ra and Rq) for the specimens. For all five materials, the control groups showed the lowest Ra and Rq, which increased with aging. Before aging, the Ra values of P were the highest; the Ra values of E were similar to those of T and lower than those of L, M, and P. Following first and second aging, the Ra values of P were higher than those of M, T, and E and lower than those of L. After the first aging cycle, E showed values similar to those of M and T and lower than those of L and P. After the second aging period, E showed values similar to those of T, higher than those of M, and lower than those of L and P. Overall, the Rq values showed similar tendency as Ra values. P showed the highest Rq values; the Rq values of E were similar to those of T and lower than those of L, M, and P. Following first and second aging, the Rq values of P were higher than those of M, T, and E, and lower than those of L. Following first and second aging, the Rq values of E were similar to those of M and T and lower than those of L and P. The independent samples t-test results revealed that the surface roughness of all groups increased significantly with aging (P < 0.05).
Fig. 8.
The mean ± standard deviation values and statistical analysis of the surface roughness (Ra and Rq) of all specimens in the groups. a CLSM and b AFM. L, 3Y-TZP of IPS E.max ZirCAD LT; M, 4Y-TZP of IPS E.max ZirCAD MT; T, 5Y-TZP of IPS E.max ZirCAD MT Multi; P, 3Y/5Y-TZP of IPS E.max ZirCAD Prime; E, 4Y/5Y-TZP of IPS E.max ZirCAD Prime esthetic. All data are presented as mean ± standard deviation values. *denotes a significant difference at P < 0.05
Representative AFM images of all five groups are shown in Fig. 8b. The mean values, standard deviations, and statistical analysis results for Ra and Rq are summarized in Supplementary Table 10. Before aging, the Ra values of P were similar to those of M, higher than those of T and E, and lower than those of L. After first and second aging, the Ra values of P were higher than those of M, T, and E and lower than those of L. The Ra values of E were similar to those of T and lower than those of L, M, and P in the control groups. After first aging, the Ra values of E were comparable to those of M and lower than those of L, T, and P. Additionally, after second aging, the Ra values of E were the lowest among the five groups tested. Before aging, the Rq values of P were similar to those of M and T, higher than those of E, and lower than those of L. Additionally, the Rq values of P were higher than those of M, T, and E, and lower than those of L following first and second aging. The Rq values of E were similar to those of T and lower than those of L, M, and P in the control and first-aged groups. In addition, the Rq values of E after the second aging period were the lowest among the five groups analyzed.
Mean ± standard deviation values and statistical analysis of surface roughness (Sa and Sq) of all specimens in the groups using AFM are exhibited in Supplementary Figure 1. The Sa and Sq values exhibited similar tendencies as Ra and Rq. Before aging, the Sa values of P were similar to those of M, higher than those of T and E, and lower than those of L. After first and second aging, the Sa values of P were higher than those of M, T, and E, and lower than those of L. The Sa values of E were comparable to those of T and lower than those of L, M, and P in the control groups. After first aging, the Sa values of E were similar to those of T and lower than those of L, M, and P. Additionally, the Sa values of E after second aging were the lowest among the five groups analyzed. Before aging, the Sq values of P were similar to those of M and T, higher than those of E, and lower than those of L. Additionally, the Sq values of P were higher than those of M, T, and E and lower than those of L following first and second aging. The Sq values of E were similar to those of T and lower than those of L, M, and P in the control and first-aged groups. Moreover, the Sq values of E after second aging were the lowest among the five groups analyzed. The independent samples t-test results revealed that the Sa and Sq values of all groups increases significantly with aging (P < 0.05).
XRD data of the various zones of all tested groups are shown in Fig. 9a. The tetragonal phase (t-phase) was predominant in control groups, and the monoclinic phase (m-phase) was hardly detectable according to XRD spectra. All five specimen groups exhibited similar diffraction peak positions corresponding to the t-phase. Hydrothermal aging in an autoclave triggered a rise in the intensity of the monoclinic () peak, which represented the most stable monoclinic structure, while inducing t → m transition, resulting in a rise in the intensity of the monoclinic (200) peak. XRD analysis indicated that all groups showed an increase in the monoclinic phase (m-phase) on aging. Notably, a greater monoclinic phase increment was observed in L and P than in M, T, and E. Figure 9b and Supplementary Table 11 showed the variation in Fm with aging based on XRD data. Before aging, L showed the highest Fm values followed by M, T, P, and E (in descending order), and following first and second aging, L showed the highest Fm values followed by P, M, T, and E (in descending order).
Fig. 9.
Phase transformation analyses in accordance with aging time. a Representative XRD patterns and b Variation in the monoclinic volume fraction (Fm). L, 3Y-TZP of IPS E.max ZirCAD LT; M, 4Y-TZP of IPS E.max ZirCAD MT; T, 5Y-TZP of IPS E.max ZirCAD MT Multi; P, 3Y/5Y-TZP of IPS E.max ZirCAD Prime; E, 4Y/5Y-TZP of IPS E.max ZirCAD Prime esthetic
FE-SEM images revealed the surface microstructures of the sample groups (Fig. 10). Before and after aging, the grain sizes were larger in materials with a higher proportion of yttria; M, T, and E contained larger grains than L and P. Notably, the surfaces of all materials subjected to hydrothermal aging contained defects such as microcracks that occurred along grain boundaries and pull-out of grains; these types of voids were particularly evident in L and P.
Fig. 10.

FE-SEM images showing the surface topography of all the specimens in the groups. L, 3Y-TZP of IPS E.max ZirCAD LT; M, 4Y-TZP of IPS E.max ZirCAD MT; T, 5Y-TZP of IPS E.max ZirCAD MT Multi; P, 3Y/5Y-TZP of IPS E.max ZirCAD Prime; E, 4Y/5Y-TZP of IPS E.max ZirCAD Prime esthetic. The white arrows indicate surface uplifts, microcracks, and irregular defects after aging
Supplementary Table 12 exhibited the weight percent of the surface compositions of specimens in the IPS E.max ZirCAD control groups using EDS. Before aging, the Y content was highest in T (6.55 ± 0.17 wt%), followed by E (5.20 ± 0.45 wt%), M (4.66 ± 0.48 wt%), L (2.97 ± 0.09 wt%), and P (2.96 ± 0.10 wt%). On comparing the surface compositions of specimens in all groups during the aging process, statistically significant differences among the materials were found for several elements (Fig. 11 and Supplementary Table 13). In all five groups, Zr was the most abundant constituent element followed by O, Y, Hf, and Al before aging. Independent samples t-test results indicated changes in the content of these elements on aging. The Y content of L and M showed no significant changes on aging (P > 0.05); however, the content of other elements showed significant changes on aging (P < 0.05). Similarly, on aging, there were no significant changes in the Zr and Hf content of T; however, the content of other elements showed significant changes on aging. In P, all five elements showed significant changes on aging, and the Zr content of the second-aged group is significantly higher than that of the control group. The O content decreased significantly after first aging, and the Y content of the control and first-aged groups as well as the control and second-aged groups were significantly different. On aging, the Al content of E showed no significant changes, whereas the content of the other elements showed varying degrees of change.
Fig. 11.
Elemental analysis of the groups using EDS. a zirconium, b oxygen, c yttrium, d hafnium, and e aluminum. L, 3Y-TZP of IPS E.max ZirCAD LT; M, 4Y-TZP of IPS E.max ZirCAD MT; T, 5Y-TZP of IPS E.max ZirCAD MT Multi; P, 3Y/5Y-TZP of IPS E.max ZirCAD Prime; E, 4Y/5Y-TZP of IPS E.max ZirCAD Prime esthetic. All data are presented as mean ± standard deviation values. *denotes a significant difference at P < 0.05
Supplementary Table 14 summarizes the Two-way ANOVA results for the surface characteristics of all specimen groups. Significant interactions existed between the aging time and yttria content for the surface roughness measured through CLSM and AFM (P < 0.05) and EDS elemental analysis (P < 0.05) for the different specimen zones.
Discussion
This in vitro study evaluated the alterations in the mechanical and surface characteristics of the transition zone of multilayered TZ compared to zones of different yttria content, after hydrothermal aging. Statistical analyses revealed that mechanical and surface properties of P and E changed following aging. Statistical analyses results presented that the mechanical and surface properties of P and E changed after aging. Therefore, the first null hypothesis that no significant variation exists in the mechanical and surface characteristics across different compositional zones before and after hydrothermal aging was rejected. Previous studies revealed that as the proportion of yttria increases, the cubic phase content rises and amount of tetragonal phase decreases. This leads to a lower possibility of tetragonal to monoclinic phase transformation, resulting in compromised strength and fracture toughness [8, 45]. Thus, mechanical properties of 3Y-TZP are superior to those of 4Y-TZP and 5Y-TZP [14, 15]. These findings conform to the findings of this study, in which L showed the highest flexural strength. Thus, the second null hypothesis that the gradient distribution of yttria content across multilayered zirconia does not significantly influence the mechanical and surface characteristics was also rejected. The third null hypothesis that the mechanical and surface characteristics of gradient zones in TZ after hydrothermal aging are not influenced by their yttria content was rejected, except for 4-point bending flexural strength and biaxial flexural strength. Several studies have insisted that the mechanical and surface characteristics of multilayered TZ were altered following hydrothermal aging [41, 46, 47]. Tetragonal to monoclinic phase transformation, which occurs in the presence of water at moderate temperature, such as in the human oral environment, is responsible for hydrothermal degradation. Therefore, 3Y-TZP suffers the most sensitive effect of hydrothermal aging, with increased amount of monoclinic phase and compromised mechanical and surface characteristics [37, 38]. Conversely, higher yttria content and the increased amount of cubic phase resulted in better resistance to aging in 5Y-TZP and 4Y-TZP. These findings conform to the results of this study. Finally, the fourth null hypothesis that no correlation exists between the 4PBFS and BFS of zones consisted of various amounts of yttria was also rejected. Previous study on the layer characteristics of multilayered TZ revealed that the characteristic strength of 4PBFS and BFS were positively correlated [12]. This is in line with the result of this study, where 4PBFS and BFS showed coefficient of correlation close to 1.0 before and after aging.
Aging occurs slowly in the oral environment, which involves exposure to various stresses, including humidity, pH variations, and mechanical loading. Current in vitro studies have failed to simulate the aging of zirconia at body temperature (37 °C) [33]. To stimulate LTD, various studies have attempted to accelerate the aging of zirconia using thermocycling [35]. Notably, the absence of a standardized protocol makes the precise analysis of zirconia aging challenging. ISO/TS 11405 suggests using two water baths at temperatures within 5–55 °C and the dwell time of at least 20 s [48]. However, the temperature in the oral cavity is regulated to maintain homeostasis at 37 °C, and significant temperature variations are not caused by eating and drinking [49]. Recent studies have identified autoclave aging with temperature, dwell time, and pressure as controlled variables to be an effective method for accelerating aging. According to Chevalier et al., 1 h of steam sterilization at 134 °C in an autoclave is equivalent to 3–4 years of aging in vivo [26]. Zirconia ceramics undergo <25% tetragonal-to-monoclinic phase transformation, which is an acceptable level of transformation according to ISO 13356:2015 [50]. The results of this study suggested that increasing the aging time promotes active t → m transformation and increases the monoclinic phase fraction in the system, especially in 3Y- and 3Y/5Y-TZP. Interestingly, L and P contain monoclinic fractions of 4.03% and 3.97%, respectively, which are below clinically acceptable limits. Because zirconia prostheses in the oral cavity are continuously in contact with water, considering the effects of hydrothermal aging on them is critical. To comprehensively understand the properties of multilayered TZ, the effect of hydrothermal aging on the mechanical and surface properties of transition zones comprising 3Y/5Y-TZP and 4Y/5Y-TZP must be compared with the properties of zones comprising 3Y-,4Y-, and 5Y-TZP.
As ceramics are brittle materials, good mechanical properties are vital in hindering crack progression and maintaining the long-lasting durability of dental prostheses. Manufacturers claim that the flexural strength describes the mechanical properties of zirconia, and materials with high flexural strength are more resistant to fracture. The slope of the Weibull probability plot, represented by the Weibull modulus (β), reflects the consistency and reliability of the measured data. A higher β value indicates increased uniformity among the data points, suggesting reduced variability in fracture strength and, consequently, higher material reliability. Conversely, a lower β value implies greater data dispersion, reflecting less predictable and more heterogeneous mechanical performance. In a Weibull probability plot, the X-axis represents the measured strength values (e.g., MPa), while the Y-axis indicates the cumulative probability of failure. A tighter clustering of data points along a steeper line suggests that the material exhibits more consistent fracture strength under the given condition. The biaxial flexural test is known to provide more reliable measurements than the 4- and 3-point bend tests because the maximum stress value is positioned at the center of the specimen, reducing the effects of edge defects [24]. This is in agreement with the results of this study; the Weibull modulus of BFS, a standard indicating the reliability of a material, is higher than that of the 4PBFS.
In addition, for all five materials used in this study, the BFS values are higher than the 4PBFS values before and after aging. The presence of edge defects can explain the lower flexural strength measured in the 4PBFS tests. Moreover, the 4PBFS and BFS values of L and P are significantly higher than those of M, T, and E before and after aging. Thus, the findings of this study conform to those of previous studies, which indicate that a higher t-ZrO2 phase content results in higher flexural strength in Y-TZP ceramics [21]. The Weibull modulus of BFS is the highest for L and lowest for E, possibly due to microstructural heterogeneity, which results from compositional variation and causes an irregular stress distribution under uniaxial loads [40], leading to a flexural strength reduction. In contrast, the Weibull modulus of the 4PBFS is the highest in M before aging and the highest in T and L after 5 and 10 h of aging, respectively. This implies that the 4PBFS test results are affected by some other factor (besides the yttria content or amount of the t-ZrO2 phase).
Pearson correlation coefficients between 4PBFS and BFS after aging showed relatively low values in the 4Y/5Y-TZP transition zone (E). Several factors may explain this reduction. The transition zone consists of a compositional gradient of tetragonal and cubic phases. Such heterogeneity can produce variable stress distributions depending on the testing mode. Aging-induced phase changes, particularly localized tetragonal-to-monoclinic transformation, may further exacerbate this heterogeneity and contribute to the discrepancy between 4PBFS and BFS. In addition, the interface between 4Y-rich and 5Y-rich regions may act as a mechanically weak zone under cyclic aging [12]. This interfacial weakening could alter the crack propagation pathway differently under uniaxial loading (4PBFS) compared with biaxial loading (BFS), thereby lowering the correlation between the two test results. While BFS applies radially uniform stress across the disk, 4PBFS induces directional tensile stress at the lower surface [51]. If the transition zone exhibits anisotropic grain orientation or residual stress patterns, the two testing modes may capture different failure mechanisms, ultimately resulting in reduced correlation after aging.
Thus, these two flexural strength tests and their correlation should be investigated further. Here, none of the five groups showed statistically significant differences between the control and aged groups; this conforms to the results of a previous study, which compares the flexural strength of dental zirconia containing different amounts of yttria after the autoclave treatment at 134 °C and 0.2 MPa for 0, 5, and 10 h [41].
Nanoindentation and Young’s modulus tests could be good techniques for characterizing the degradation of zirconia surfaces on hydrothermal aging; the degradation can be estimated by analyzing the reduction in hardness and Young’s modulus with penetration depth [52]. In this study, the nanoindentation hardness and Young’s modulus of M and T were the highest before and after aging, as expected for brittle 4Y,5Y-TZP; similar results were found in a previous study, which reports that Katana UTML and STML, comprising 5Y- and 4Y-TZP, respectively, showed extremely high values of nanoindentation hardness [41]. The nanoindentation hardness of L, M, and P undergoes reduction on aging; the reduction is the most significant for L and P, possibly owing to the formation of microcracks due to volumetric expansion on t–m transformation during hydrothermal aging. Microcracks adversely affect the hardness and Young’s modulus of zirconia systems [53].
In this study, the Vickers microhardness, which is associated with resistance to abrasion, showed a statistically significant reduction in all materials on hydrothermal aging. This is in line with the results of a previous study in that aging compromises the Vickers hardness of zirconia stabilized with yttria [54]. Here, E exhibits the highest Vickers hardness values before aging, while T and M exhibited the highest values after 5 and 10 h of aging, respectively.
Surface characteristics analyses showed that zirconia containing different amounts of yttria is influenced by hydrothermal aging. CLSM and AFM were conducted to investigate the surface roughness of the specimens, while XRD was used to assess their phase distribution, SEM was used to analyze their surface microstructure, and EDS was used for elemental composition analysis. Surface roughness and microstructure characteristics can affect the strength of dental prostheses and are associated with their appearance, final color, and bacterial accumulation [8]. In this study, the surface roughness values of all the tested materials increased on hydrothermal aging. L showed higher surface roughness values after aging than M and T, indicating that a low yttria content facilitates tetragonal to monoclinic phase transformation, resulting in abundant grain pull-out and surface irregularities. Interestingly, zirconia stabilized with a higher yttria content showed higher resistance to hydrothermal aging [33, 41]. According to the literature, Ra values larger than 0.2 μm increase the possibility of bacterial deposition, and a roughness of 0.25–0.50 μm can be detected by the tongue. All specimens in this study showed roughness values below 0.1 μm, which is within the clinically acceptable range, even after aging.
XRD phase-distribution analysis indicated that L and P undergo a tetragonal-to-monoclinic phase transformation, as indicated by the presence of monoclinic peaks in the XRD spectra of the relevant specimens. M, T, and E contain low amounts of the monoclinic phase, even after 10 h of hydrothermal aging, indicating resistance toward phase transformation. 4Y-and 5Y-TZP contain a lower amount of the monoclinic phase than 3Y-TZP; thus, these results are consistent with previous reports [41, 47]. Moreover, the results of phase distribution analysis based on XRD data are consistent with the increased surface roughness values observed in this study, as tetragonal-to-monoclinic phase transformation induces volume expansion, leading to a surface uplift and pull-out of grains [31, 36]. The final heat treatment of Y-TZP specimens at 900–1000 °C for 1 h leads to reverse transformation from the monoclinic to the tetragonal phase, resulting in a low proportion of the monoclinic phase in the control group.
SEM and EDS analyses indicated surface uplift, grain pull-out, and irregular defects in all five materials used in this study, particularly in the L and P samples, possibly owing to changes in the elemental composition of the specimens with aging. Currently, changes in the elemental composition of yttria-stabilized zirconia remain largely unexplored; future research should focus on investigating the reason for the variation observed in the content of different elements in such systems on hydrothermal aging. E showed a surface microstructure similar to that of T, with larger grain sizes, possibly due to a high proportion of the cubic phase.
The surface microstructure and phase distribution of P are comparable to those of L under all aging conditions. However, after aging, the surface roughness values of P are lower than those of L and higher than those of M, T, and E. In addition, the surface microstructure and phase distribution of E are comparable to those of T under all aging conditions. After aging, the surface roughness values of E are lower than or similar to those of T.
One of the limitations of this study is that autoclave aging method at 134 °C/0.2 MPa cannot precisely simulate the dynamic loading, temperature changes, and salivary pH fluctuations occurring in the human oral cavity. Also, restricting specimen preparation to a single horizontal orientation does not account for potential variations that might occur if specimens were prepared vertically across multiple layers. Such differences could influence stress distribution, crack propagation pathways, and overall flexural reliability. Future studies should evaluate the impact of vertical milling across compositional gradients to fully address the role of mechanical anisotropy in multilayered zirconia. Furthermore, while autoclave aging at 134 °C/0.2 MPa is an accepted acceleration method for simulating low-temperature degradation (LTD), it does not replicate the multi-factorial aging process observed in the oral cavity, which involves thermocycling, salivary pH fluctuations, and repeated mechanical loading [25, 46]. Future investigations should incorporate fatigue testing, pH-controlled environments, and dynamic thermocycling protocols (e.g., 5–55 °C, 10,000 20,000 cycles) to better simulate intraoral aging conditions. Also, in vivo studies probing the longevity of restorations made from multilayered TZ should be conducted. Furthermore, the aging time was limited to 10 h in this study, and changes in flexural strength did not occur within this time. Because 10 h of autoclave aging is equivalent to ~30 years of clinical use, future studies should investigate the influence of a longer aging time on flexural strength. Additionally, further research should determine how the optical properties of TZ are influenced by an increase in surface roughness resulting from the aging process. Moreover, the optical properties and biocompatibility of the transition zone of IPS E.max ZirCAD Prime Esthetic should be explored in comparison with zones containing different amounts of yttria.
Conclusions
The following conclusions can be derived from the results of this in vitro study:
The 4PBFS of 3Y/5Y-TZP is similar to that of 3Y-TZP; however, the BFS of 3Y/5Y-TZP is lower than that of 3Y-TZP, both before and after aging. The 4PBFS and BFS of 4Y/5Y-TZP are similar to those of 4Y-TZP and 5Y-TZP, both before and after aging.
The 4PBFS of zones containing different amounts of yttria before and after aging are correlated with their BFS. Neither type of flexural strength exhibits significant differences based on yttria content after aging.
The stiffness and surface hardness of 3Y-TZP are lower than those of 4Y-TZP and 5Y-TZP. Both properties exhibit significant differences based on yttria content after aging.
On aging, the surface roughness increases in all five groups, with the highest increase observed in the 3Y-TZP group. However, the roughness of the tested specimens is within the clinically acceptable range (Ra < 0.2 µm).
On aging, the occurrence of grain pull-out, microcracks, and irregular defects in 3Y-TZP and 3Y/5Y-TZP is higher than that in 4Y-TZP, 5Y-TZP, and 4Y/5Y-TZP owing to more phase transformation (t → m) in 3Y-TZP and 3Y/5Y-TZP.
The surface roughness and hardness showed significant differences based on yttria content after aging.
The phase composition and surface microstructure of 3Y/5Y-TZP and 4Y/5Y-TZP resembled those of 3Y-TZP and 5Y-TZP, respectively.
The mechanical and surface properties of different zones of translucent monolithic zirconia are expected to be influenced by yttria content after hydrothermal aging.
From a clinical standpoint, the 3Y/5Y-TZP transition zone exhibited consistently high flexural strength and satisfactory aging resistance, supporting its use in posterior restorations where mechanical durability is critical. In contrast, the 5Y-TZP and 4Y/5Y-TZP zones demonstrated lower strength and greater variability, suggesting their suitability for anterior restorations subjected to reduced masticatory loads. When positioning the CAD design of an anterior restoration within a multilayered zirconia block, the relative proportions of the incisal, transition, and dentin zones should be carefully considered, recognizing that the mechanical performance of the 4Y/5Y-TZP layer is comparable to that of 5Y-TZP. These findings may assist clinicians in determining optimal milling positions during the CAD/CAM fabrication of multilayered zirconia restorations.
Supplementary information
Acknowledgements
This work was supported by the National Research Foundation of Korea (NRF) grant funded by the Korea government (MSIT) [NRF-2021R1F1A1048462, RS-2023-00253926], by Medical Research Center Program [NRF-2021R1A5A2022318].
Compliance with ethical standards
Conflict of interest
The authors declare no competing interests.
Footnotes
Publisher’s note Springer Nature remains neutral with regard to jurisdictional claims in published maps and institutional affiliations.
Contributor Information
Jin-Soo Ahn, Email: ahnjin@snu.ac.kr.
Yu-Sung Choi, Email: choiys@dankook.ac.kr.
Supplementary information
The online version contains supplementary material available at 10.1007/s10856-025-06938-8.
References
- 1.Zhang Y, Lawn BR. Novel zirconia materials in dentistry. J Dent Res. 2018;97:140–7. 10.1177/0022034517737483 [DOI] [PMC free article] [PubMed] [Google Scholar]
- 2.McLaren EA, Maharishi A, White SN. Influence of yttria content and surface treatment on the strength of translucent zirconia materials. J Prosthet Dent. 2023;129:638–43. 10.1016/j.prosdent.2021.07.001 [DOI] [PubMed] [Google Scholar]
- 3.Flask JD, Thompson GA, Singh M, Berzins DW. Edge chipping of TZ. J Prosthet Dent. 2022;127:793–800. 10.1016/j.prosdent.2020.12.009 [DOI] [PubMed] [Google Scholar]
- 4.Denry I, Kelly JR. State of the art of zirconia for dental applications. Dent Mater. 2008;24:299–307. 10.1016/j.dental.2007.05.007 [DOI] [PubMed] [Google Scholar]
- 5.Zhang F, Inokoshi M, Batuk M, Hadermann J, Naert I, Van Meerbeek B, Vleugels J. Strength, toughness and aging stability of highly-translucent Y-TZP ceramics for dental restorations. Dent Mater. 2016;32:e327–37. 10.1016/j.dental.2016.09.025 [DOI] [PubMed] [Google Scholar]
- 6.Zhang F, Van Meerbeek B, Vleugels J. Importance of tetragonal phase in high-translucent partially stabilized zirconia for dental restorations. Dent Mater. 2020;36:491–500. 10.1016/j.dental.2020.01.017 [DOI] [PubMed] [Google Scholar]
- 7.Zhang Y. Making yttria-stabilized tetragonal zirconia translucent. Dent Mater. 2014;30:1195–203. 10.1016/j.dental.2014.08.375 [DOI] [PMC free article] [PubMed] [Google Scholar]
- 8.Toma FR, Bîrdeanu MI, Uțu I-D, Vasiliu RD, Moleriu LC, Porojan L. Surface characteristics of high translucent multilayered dental zirconia related to aging. Materials. 2022;15:3606. 10.3390/ma15103606 [DOI] [PMC free article] [PubMed] [Google Scholar]
- 9.Jerman E, Lumkemann N, Eichberger M, Zoller C, Nothelfer S, Kienle A, Stawarczyk B. Evaluation of translucency, Marten’s hardness, biaxial flexural strength and fracture toughness of 3Y-TZP, 4Y-TZP and 5Y-TZP materials. Dent Mater. 2021;37:212–22. 10.1016/j.dental.2020.11.007 [DOI] [PubMed] [Google Scholar]
- 10.Ban S. Classification and properties of dental zirconia as implant fixtures and superstructures. Materials. 2021;14:4879. 10.3390/ma14174879 [DOI] [PMC free article] [PubMed] [Google Scholar]
- 11.Michailova M, Elsayed A, Fabel G, Edelhoff D, Zylla I-M, Stawarczyk B. Comparison between novel strength-gradient and color-gradient multilayered zirconia using conventional and high-speed sintering. J Mech Behav Biomed Mater. 2020;111:103977. 10.1016/j.jmbbm.2020.103977 [DOI] [PubMed] [Google Scholar]
- 12.Inokoshi M, Liu H, Yoshihara K, Yamamoto M, Tonprasong W, Benino Y, Minakuchi S, Vleugels J, Van Meerbeek B, Zhang F. Layer characteristics in strength-gradient multilayered yttria-stabilized zirconia. Dent Mater. 2023;39:430–41. 10.1016/j.dental.2023.03.015 [DOI] [PubMed] [Google Scholar]
- 13.Kolakarnprasert N, KaiEr MR, Kim DK, Zhang Y. New multi-layered zirconias: composition, microstructure and translucency. Dent Mater. 2019;35:797–806. 10.1016/j.dental.2019.02.017 [DOI] [PMC free article] [PubMed] [Google Scholar]
- 14.Strasser T, Schmid A, Huber C, Rosentritt M. 4-Unit Molar fixed partial dentures made from highly translucent and multilayer zirconia materials: an in vitro investigation. Ceramics. 2022;5:99–107. 10.3390/ceramics5010009 [Google Scholar]
- 15.Strasser T, Wertz M, Koenig A, Koetzsch T, Rosentritt M. Microstructure, composition, and flexural strength of different layers within zirconia materials with strength gradient. Dent Mater. 2023;39:463–8. 10.1016/j.dental.2023.03.012 [DOI] [PubMed] [Google Scholar]
- 16.Marini G, da Rosa LS, Machado PS, Silvestre FA, Valandro LF, Feitosa VP, Pereira GKR, Bacchi A. Fatigue performance analysis of strength-graded zirconia polycrystals for monolithic three-unit implant-supported prostheses. J Mech Behav Biomed Mater. 2023;140:105736. 10.1016/j.jmbbm.2023.105736 [DOI] [PubMed] [Google Scholar]
- 17.Cesar PF, de Paula Miranda RB, Santos KF, Scherrer SS, Zhang Y. Recent advances in dental zirconia: 15 years of material and processing evolution. Dent Mater. 2024;40:824–36. 10.1016/j.dental.2024.02.026 [DOI] [PMC free article] [PubMed] [Google Scholar]
- 18.Kaizer MR, Kolakarnprasert N, Rodrigues C, Chai H, Zhang Y. Probing the interfacial strength of novel multi-layer zirconias. Dent Mater. 2020;36:60–7. 10.1016/j.dental.2019.10.008 [DOI] [PMC free article] [PubMed] [Google Scholar]
- 19.Pereira RM, Campos TMB, Bonfante EA, Thim GP. A comparative study of mechanical properties of yttria stabilized zirconia monolithic and bilayer configuration for dental application. J Mech Behav Biomed Mater. 2023;148:106160. 10.1016/j.jmbbm.2023.106160 [DOI] [PubMed] [Google Scholar]
- 20.Vardhaman S, Borba M, KaiEr MR, Kim DK, Zhang Y. Optical and mechanical properties of the multi‐transition zones of a TZ. J Esthet Restor Dent. 2024;0:1–8. 10.1111/jerd.13319 [DOI] [PMC free article] [PubMed] [Google Scholar]
- 21.Labetić A, Klaser T, Skoko Ž, Jakovac M, Žic M. Flexural strength and morphological study of different multilayer zirconia dental materials. Materials. 2024;17:1143. 10.3390/ma17051143 [DOI] [PMC free article] [PubMed] [Google Scholar]
- 22.Bakitian F. Flexural strength of TZ materials produced with different multilayer technologies: an in vitro study. Int J Dent. 2024;2024:8410101. 10.1155/2024/8410101 [DOI] [PMC free article] [PubMed] [Google Scholar]
- 23.Jeong HY, Lee HH, Choi YS. Mechanical properties of hybrid computer-aided design/computer-aided manufacturing (CAD/CAM) materials after aging treatments. Ceram Int. 2018;44:19217–26. 10.1016/j.ceramint.2018.07.146 [Google Scholar]
- 24.Alghazzawi TF, Janowski GM, Eberhardt AW. An experimental study of flexural strength and hardness of zirconia and their relation to crown failure loads. J Prosthet Dent. 2024;131:320–8. 10.1016/j.prosdent.2022.04.005 [DOI] [PubMed] [Google Scholar]
- 25.ISO 6872:2015, Dentistry—Ceramic Materials, International Organization for Standardization, Geneva, Switzerland, https://www.iso.org/standard/59936.html, 2015 (accessed October 2023).
- 26.Chevalier J, Cales B, Drouin JM. Low‐temperature aging of Y‐TZP ceramics. J Am Ceram Soc. 1999;82:2150–4. 10.1111/j.1151-2916.1999.tb02055.x [Google Scholar]
- 27.Chevalier J. What future for zirconia as a biomaterial? Biomaterials. 2006;27:535–543. 10.1016/j.biomaterials.2005.07.034 [DOI] [PubMed] [Google Scholar]
- 28.Deville S, Chevalier J, Gremillard L. Influence of surface finish and residual stresses on the ageing sensitivity of biomedical grade zirconia. Biomaterials. 2006;27:2186–92. 10.1016/j.biomaterials.2005.11.021 [DOI] [PubMed] [Google Scholar]
- 29.Ramesh S, Lee KS, Tan C. A review on the hydrothermal ageing behaviour of Y-TZP ceramics. Ceram Int. 2018;44:20620–34. 10.1016/j.ceramint.2018.08.216 [Google Scholar]
- 30.Lughi V, Sergo V. Low temperature degradation-aging-of zirconia: a critical review of the relevant aspects in dentistry. Dent mater. 2010;26:807–20. 10.1016/j.dental.2010.04.006 [DOI] [PubMed] [Google Scholar]
- 31.De Souza GM, Zykus A, Ghahnavyeh RR, Lawrence SK, Bahr DF. Effect of accelerated aging on dental zirconia-based materials. J Mech Behav Biomed Mater. 2017;65:256–63. 10.1016/j.jmbbm.2016.08.023 [DOI] [PubMed] [Google Scholar]
- 32.Muñoz EM, Longhini D, Antonio SG, Adabo GL. The effects of mechanical and hydrothermal aging on microstructure and biaxial flexural strength of an anterior and a posterior monolithic zirconia. J Dent. 2017;63:94–102. 10.1016/j.jdent.2017.05.021 [DOI] [PubMed] [Google Scholar]
- 33.Kim HK, Kim SH. Effect of hydrothermal aging on the optical properties of precolored dental monolithic zirconia ceramics. J Prosthet Dent. 2019;121:676–82. 10.1016/j.prosdent.2018.06.021 [DOI] [PubMed] [Google Scholar]
- 34.Chevalier J, Deville S, Münch E, Jullian R, Lair F. Critical effect of cubic phase on aging in 3 mol% yttria-stabilized zirconia ceramics for hip replacement prosthesis. Biomaterials. 2004;25:5539–45. 10.1016/j.biomaterials.2004.01.002 [DOI] [PubMed] [Google Scholar]
- 35.Flinn BD, Raigrodski AJ, Singh A, Mancl LA. Effect of hydrothermal degradation on three types of zirconias for dental application. J Prosthet Dent. 2014;112:1377–84. 10.1016/j.prosdent.2014.07.015 [DOI] [PubMed] [Google Scholar]
- 36.Kim JW, Covel N, Guess P, Rekow E, Zhang Y. Concerns of hydrothermal degradation in CAD/CAM zirconia. J Dent Res. 2010;89:91–5. 10.1177/0022034509354193 [DOI] [PMC free article] [PubMed] [Google Scholar]
- 37.Amarante JEV, Pereira MVS, De Souza GM, Alves MFRP, Simba BG, Dos Santos C. Effect of hydrothermal aging on the properties of zirconia with different levels of translucency. J Mech Behav Biomed Mater. 2020;109:103847. 10.1016/j.jmbbm.2020.103847 [DOI] [PubMed] [Google Scholar]
- 38.Camposilvan E, Leone R, Gremillard L, Sorrentino R, Zarone F, Ferrari M, Chevalier J. Aging resistance, mechanical properties and translucency of different yttria-stabilized zirconia ceramics for monolithic dental crown applications. Dent Mater. 2018;34:879–90. 10.1016/j.dental.2018.03.006 [DOI] [PubMed] [Google Scholar]
- 39.Lümkemann N, Stawarczyk B. Impact of hydrothermal aging on the light transmittance and flexural strength of colored yttria-stabilized zirconia materials of different formulations. J Prosthet Dent. 2021;125:518–26. 10.1016/j.prosdent.2020.01.016 [DOI] [PubMed] [Google Scholar]
- 40.UwanyuE RS, Ramesh S, King JrMK, Lawson N, Mahapatra MK. Mechanical properties, translucency, and low temperature degradation (LTD) of yttria (3–6 mol%) stabilized zirconia. Ceram Int. 2021;47:15868–74. 10.1016/j.ceramint.2021.02.161 [Google Scholar]
- 41.Ha SR, Choi YS. Effect of hydrothermal aging on dental multilayered zirconia for monolithic restorations: an in vitro study. Ceram Int. 2021;47:17057–68. 10.1016/j.ceramint.2021.03.013 [Google Scholar]
- 42.Kulyk V, Duriagina Z, Vasyliv B, Vavrukh V, Kovbasiuk T, Lyutyy P, Vira V. The effect of sintering temperature on the phase composition, microstructure, and mechanical properties of yttria-stabilized zirconia. Materials. 2022;15:2707. 10.3390/ma15082707 [DOI] [PMC free article] [PubMed] [Google Scholar]
- 43.Garvie RC, Nicholson PS. Phase analysis in zirconia systems. J Am Ceram Soc. 1972;55:303–5. 10.1111/j.1151-2916.1972.tb11290.x [Google Scholar]
- 44.Toraya H, Yoshimura M, Somiya S. Calibration curve for quantitative analysis of the monoclinic‐tetragonal ZrO2 system by X‐ray diffraction. J Am Ceram Soc. 1984;67:C‐119–21. 10.1111/j.1151-2916.1984.tb19715.x [Google Scholar]
- 45.Winter A, Schurig A, Odenthal A-L, Schmitter M. Impact of different layers within a blank on mechanical properties of multi-layered zirconia ceramics before and after thermal aging. Dent Mater. 2022;38:e147–54. 10.1016/j.dental.2022.03.009 [DOI] [PubMed] [Google Scholar]
- 46.Li Q, Yang Y, Chen K, Jiang Y, Swain MV, Yao M, He Y, Liang Y, Jian Y, Zhao K. Effect of low-temperature degradation on the fatigue performance of dental strength-gradient multilayered zirconia restorations. J Dent. 2024;142:104866. 10.1016/j.jdent.2024.104866 [DOI] [PubMed] [Google Scholar]
- 47.Choi YS, Kang KH, Att W. Effect of aging process on some properties of conventional and multilayered translucent zirconia for monolithic restorations. Ceram Int. 2020;46:1854–68. 10.1016/j.ceramint.2019.09.162 [Google Scholar]
- 48.ISO/TS 11405:2015, Dentistry—Testing of adhesion to tooth structure, International Organization for Standardization, Geneva, Switzerland. https://www.iso.org/standard/62898.html, 2015 (accessed June 2019).
- 49.Gale M, Darvell B. Thermal cycling procedures for laboratory testing of dental restorations. J Dent. 1999;27:89–99. 10.1016/S0300-5712(98)00037-2 [DOI] [PubMed] [Google Scholar]
- 50.ISO 13356:2015, Dentistry—Implants for surgery—Ceramic materials based on yttria-stabilized tetragonal zirconia (Y-TZP), International Organization for Standardization, Geneva, Switzerland. https://www.iso.org/standard/62373.html, 2015 (accessed May 2024).
- 51.Hjerppe J, Närhi TO, Vallittu PK, Lassila LV. Surface roughness and the flexural and bend strength of zirconia after different surface treatments. J Prosthet Dent. 2016;116:577–83. 10.1016/j.prosdent.2016.02.018 [DOI] [PubMed] [Google Scholar]
- 52.Gaillard Y, Jiménez-Piqué E, Soldera F, Mücklich F, Anglada M. Quantification of hydrothermal degradation in zirconia by nanoindentation. Acta Mater. 2008;56:4206–16. 10.1016/j.actamat.2008.04.050 [Google Scholar]
- 53.Monzavi M, Zhang F, Douillard T, Gremillard L, Noumbissi S, Nowzari H, Chevalier J. Microstructural analyses of artificial ageing in 5 commercially and non-commercially available Zirconia dental implants. J Eur Ceram Soc. 2020;40:3642–55. 10.1016/j.jeurceramsoc.2020.03.050 [Google Scholar]
- 54.Cattani-Lorente M, Scherrer SS, Ammann P, Jobin M, Wiskott HA. Low temperature degradation of a Y-TZP dental ceramic. Acta Biomater. 2011;7:858–65. 10.1016/j.actbio.2010.09.020 [DOI] [PubMed] [Google Scholar]
Associated Data