Abstract
Objective
The goal of this study was to test and compare how well three modern composite materials – Charisma Classic (Kulzer), G-ænial Anterior (GC Corporation) and Omnichroma (Tokuyama) – adhere to enamel surfaces that were prepared in the same way for all three of them.
Materials and method
Fifteen human teeth were extracted out, cleaned and kept in isotonic saline for the study. Before the adhesive system was applied, the enamel surfaces were etched with 37% phosphoric acid, cleaned and dried. Each composite was poured into standardised cylindrical moulds (3 mm diameter, 3 mm height) and light-cured for 40 seconds. The specimens were placed in epoxy resin and evaluated using an Instron 8872 universal testing equipment to determine shear bond strength. Five tests were conducted on each material and the mean results were identified by leaving out the outliers.
Results
G-ænial Anterior had the highest average SBS value (about 341 N), followed by Omnichroma (about 269 N) and Charisma Classic (about 266 N). Notably, two G-ænial samples showed cohesive fractures within the composite, which means that the bonds between the different parts are very strong. Most of the time, the Charisma and Omnichroma samples failed to adhere at the tooth-composite interface.
Conclusions
G-ænial Anterior had the best adhesion to enamel among all examined materials. This was shown by both the bond strength and the way the bond failed. The results indicate that using it in high-stress clinical situations may make it work more effectively and last longer. Even though Charisma Classic and Omnichroma demonstrated steady and moderate adherence, improved adhesive procedures might help them achieve the best possible clinical results.
Keywords: G-ænial Anterior, direct restorations, enamel bonding, composite resins, dental adhesion, shear bond strength
INTRODUCTION
Adhesion is defined as the bonding force that is established between two different materials at the level of their contact surfaces. This force may be physical (Van der Waals interactions, electrostatic forces), mechanical (microstructural anchoring), or chemical (ionic or covalent bonds). In the context of direct restorations, adhesion is the key factor that determines the longevity and stability of the restoration (1).
Adhesion of composite materials to enamel and dentin is governed by a combination of mechanical, chemical and micromorphological factors. For enamel, effective adhesion is mainly obtained by a micro-mechanical anchoring mechanism generated by the action of the ortho-phosphoric acid used in the surface treatment that creates micropores in the mineralized surface. Adhesive application allows the resin to penetrate these micropores, followed by photopolymerization, thus forming a stable interpenetrating network (2).
In contrast, at the dentin level, the complex composition, with a high proportion of water and collagen, makes adhesion more difficult to achieve. Adhesion to dentin involves the formation of a hybrid layer, where hydrophilic monomers of the adhesive system infiltrate the collagen network exposed after demineralization. The process is influenced by factors such as substrate moisture, adhesive system and chemical pretreatment (3, 4).
Currently, many adhesive materials are formulated as “universal adhesive” or “self-etch” systems, which contain functional monomers, such as 10-MDP (10-methacryloyloxydecyl dihydrogen phosphate), capable of establishing stable chemical bonds with calcium ions in dental hydroxyapatite (5). This chemical interaction, combined with mechanical anchorage, contributes to a durable adhesion that is resistant to degradation over time.
Adhesion of composite materials to natural tooth structure is an essential factor in the long-term success of direct restorations. The mechanical properties, application method and pre-treatments of dental surfaces directly influence the stability and durability of the bond between the restorative material and dental substrate. In particular, shear bond strength tests (SBST) are widely used to evaluate the performance of composites on enamel and dentin, due to their clinical relevance and reproducibility of the results (6, 7).
The constant progress in the development of composite materials has led to the emergence of new generations of resins with optimized chemical composition and filler particles adapted to increase the mechanical strength capacity, as well as the quality of the chemical bond with the tooth structure. Charisma Classic (Kulzer) is a microhybrid composite resin based on a Bis-GMA/TEGDMA matrix, reinforced with barium aluminum fluoride glass fillers (8). G-ænial Anterior (GC Corporation) is a radiopaque, microfilled hybrid composite that incorporates prepolymerized fillers within a UDMA-based resin matrix, enhancing polishability and wear resistance (9). On the other hand, Omnichroma (Tokuyama) is a novel single-shade composite that relies on supra-nanometer spherical fillers combined with a unique “structural color” technology, which has been designed to mimic surrounding tooth shades without additional pigments (10). These chemical and structural differences may influence the adhesion of each material to enamel and dentin, making comparative evaluation clinically relevant.
In this context, the present study investigates the adhesion of the three composite materials applied to enamel surfaces prepared under a standardized protocol, using shear bond strength tests performed with an Instron 8872 universal testing machine (11, 12). The novelty of this study lies in the direct comparison of three chemically distinct composites under identical test conditions, aiming to correlate their specific formulations with adhesive performance. This approach provides valuable insight into the clinical selection of restorative composites, particularly in situations where adhesion is a critical determinant of long-term success.
MATERIALS AND METHODS
Preparation of dental specimens
For this study, 15 extracted human teeth with therapeutic indications were collected and immediately cleaned and stored in isotonic saline to maintain hydration and prevent structural alteration (Figure 1). The teeth were collected from the private dental practices. Extractions were performed for therapeutic reasons unrelated to this research, such as advanced periodontal disease, orthodontic indications, or non-restorable carious lesions. None of the teeth were extracted specifically for the purposes of this study. After cleaning, a selected area on each tooth was prepared according to the standard dental protocol for direct restorations: mechanical cleaning, demineralization with 37% phosphoric acid, washing and drying with compressed air. This step allows the creation of a rough surface on the enamel, essential for the anchoring of the adhesive and composite material.
FIGURE 1.
Teeth stored in saline solution at approximately 10 °C
Application of composite materials
In the present study, three types of composite materials were employed, including Charisma Classic (Kulzer) – code 1_CH; G-ænial Anterior (GC Corporation) – code 2_GC; and Omnichroma (Tokuyama) – code 3_CA.
For each composite material, the adhesive system recommended by the manufacturer was used. Charisma Classic (Kulzer, Germany) was applied in association with GLUMA Bond (Kulzer), according to the manufacturer’s instructions. G-ænial Anterior (GC Corporation, Japan) was used together with G-Premio Bond (GC Corporation), while Omnichroma (Tokuyama Dental, Japan) was applied in association with Tokuyama Universal Bond (Tokuyama Dental). Adhesives were applied strictly following the manufacturers’ protocols regarding etching, application time, solvent evaporation and light-curing. The rationale for this approach was to replicate the clinical conditions recommended for each product and to allow a reliable comparison of their adhesive performance under optimal usage conditions. After application of the compatible adhesive system, each composite was applied in a uniform amount and then shaped into standardized cylinders with a diameter of approximately 3 mm and a height of 3 mm. Light-curing was performed with an LED lamp with an intensity of at least 1000 mW/cm² for 40 seconds (Figure 2).
FIGURE 2.
Macroscopic aspect of teeth prepared with the three composite materials
FIGURE 3a.

Steps for fixing teeth in epoxy resin
FIGURE 3b.

Steps for fixing teeth in epoxy resin
TABLE 1.
Coding of composite materials used in the present study

Embedding the samples
Before testing, the teeth were dried and temporarily fixed in a vertical position (Figure 3a). Each sample was then embedded in epoxy resin in a polymer cylinder (diameter 45 mm, height 10–15 mm) (Figure 3b), so that the composite area remained exposed. This method allows for easy handling and uniform fixation in the testing apparatus.
Mechanical testing
Shear tests were performed using a universal mechanical testing machine (Instron 8872), configured for shear applications and equipped with a servo-hydraulic system. The embedded samples were fixed between the jaws of the machine and a calibrated steel rod exerted force on the composite-tooth contact area at a constant speed of 1.5 mm/min (Figure 4a and 4b). Each sample was tested at room temperature, immediately after extraction from the saline solution in which it had been stored.
FIGURE 4.

INSTRON 8872 mechanical testing machine (a) and detailed image with a sample fixed in the machine's jaws and the test being performed (b)
RESULTS
Presentation of individual values and force-displacement curves
For each composite material tested, five mechanical shear tests were performed, the results being recorded as force-displacement curves. The individual curves for each group (1_CH, 2_GC, 3_CA) highlight different behaviors under mechanical stress.
Comparative analysis of the displacement strength
Table 2 presents the values recorded in the shear tests. For each group,the extreme values (minimum and maximum) were eliminated and the mean and standard deviation were calculated from the three remaining values.
TABLE 2.
Displacement force values and statistical values obtained
Qualitative and quantitative analysis of the mechanical behavior following shear tests revealed notable differences between the three composite materials used (Figure 5a, 5b, 5c).
FIGURE 5a.

Force-displacement curves obtained for all three samples
FIGURE 5b.

Force-displacement curves obtained for all three samples
FIGURE 5c.

Force-displacement curves obtained for all three samples
For material 1_CH (Charisma Classic), all five tested samples were completely detached from the tooth surface without showing cracks or internal fractures in the composite mass. The values of the detachment force ranged between 155 N and 347 N, indicating moderate adhesion, with a relatively uniform mechanical behavior and without notable extremes.
Material 2_GC (G-ænial Anterior) demonstrated the best performance among those tested. Two of the five samples (GC_a and GC_c) showed internal fractures in the composite mass, a sign that the failure did not occur at the interface with the tooth, but inside the material itself – an aspect that suggests a very strong adhesion to the dental substrate. The values recorded ranged from 144 N to 448 N, indicating a wide range of behavior, but also the highest individual value observed in the study. The average displacement force for this material was approximately 341 N, supporting the hypothesis of a high-quality bond at the material-tooth interface.
Regarding the 3_CA (Omnichroma) material, all samples displaced without cracks or fractures, similar to the behavior observed for 1_CH. The values obtained ranged from 148 N to 330 N, with an average close to 269 N, indicating an intermediate adhesion, more constant than for 2_GC, but inferior in overall performance.
The comparative analysis revealed that the 2_GC material is significantly superior in terms of adhesion, both through the high displacement force values and through the type of fracture observed. Materials 1_CH and 3_CA showed comparable and lower adhesion, without internal material fractures, indicating a weaker cohesion of the adhesive interface. These results suggest that G-ænial Anterior is able to provide a more effective bond to hard dental structures and is therefore a promising candidate for clinical use in direct restorations subjected to mechanical stress (Figure 6).
The study protocol was conducted in accordance with the ethical standards of the institutional research committee and with the 1964 Helsinki declaration and its later amendments. Informed consent was obtained from all subjects for the use of their extracted teeth in research.
FIGURE 6.

Displacement forces for the three tested materials
DISCUSSIONS
The results of the present study demonstrated a superior performance of G-ænial Anterior compared to Charisma Classic and Omnichroma in terms of shear bond strength. The average force values (~341 N) recorded for G-ænial Anterior were significantly higher than those obtained for Charisma Classic (~266 N) and Omnichroma (~269 N). Moreover, the observation that two samples from the G-ænial group failed within the composite mass, rather than at the adhesive interface, indicates that the bond to the dental substrate was stronger than the internal cohesion of the restorative material. This cohesive failure mode highlights the robustness of the adhesive mechanism and suggests favorable clinical durability.
These findings are consistent with previous investigations reporting that microhybrid composites often achieve higher bond strength to enamel compared to nanohybrid or nanofilled composites. Lahari et al (13) showed that microhybrid composites provided higher repair bond strength compared to nanohybrid and nanofilled resins, while other studies (14) confirmed that microhybrid formulations had superior adhesive performance, particularly after appropriate surface treatment. Furthermore, studies evaluating adhesion to demineralized dentin also confirm the importance of adhesive selection in influencing SBS values (15, 16).
The strong performance of G-ænial can also be attributed to its resin matrix, which incorporates functional monomers such as UDMA. Previous researches have demonstrated that adhesive systems containing functional monomers like 10-MDP establish stable chemical bonds with hydroxyapatite and maintain bond strength even after thermocycling, thereby supporting long-term durability (17).
When comparing the other two materials, Omnichroma exhibited mean bond strength values similar to Charisma Classic. Recent studies confirm that Omnichroma maintains adequate adhesive performance even after artificial aging. Elolimy et al demonstrated that thermocycling reduced bond strength for both Omnichroma and Filtek Z-350 XT, but Omnichroma experienced less degradation, suggesting promising adhesive stability (18). Similarly, Degirmenci et al reported that Omnichroma achieved the highest bond strength values among single-shade composites when repairing resin nanoceramic substrates, further highlighting its mechanical reliability (19). However, unlike G-ænial Anterior, Omnichroma did not exhibit cohesive fracture behavior, which in our study appears to be a marker of particularly strong interfacial adhesion.
From a clinical perspective, these results suggest that G-ænial Anterior is a suitable choice for direct restorations exposed to mechanical stress, due to its superior bond strength and favorable failure pattern. While Charisma Classic and Omnichroma provided moderate adhesion, their performance may still be clinically acceptable if adhesive protocols are carefully followed, emphasizing the importance of strict compliance with manufacturers’ instructions during application. At the same time, the cohesive fractures observed within the composite mass for G-ænial indicate that the intrinsic mechanical strength of the material itself also plays an important role in restoration longevity, and not only the adhesion to tooth structure.
This study has several limitations, including the relatively small number of samples (n=5 per group) and the absence of artificial aging procedures such as thermocycling, which may influence the long-term adhesive behavior. Moreover, the evaluation was restricted to shear bond strength testing, which, although widely used, may not capture all aspects of clinical performance. Recent guidelines from the Academy of Dental Materials recommend complementing shear testing with microtensile bond strength evaluations and incorporating thermal aging protocols to provide a more comprehensive assessment of adhesive stability (20). Future studies should therefore include thermocycling cycles, microtensile bond strength tests, and further analysis of the relationship between cohesive failure patterns and the specific chemical composition of each composite.
In summary, the present study confirms the superior adhesive performance of G-ænial Anterior compared to Charisma Classic and Omnichroma, while also highlighting the clinical relevance of cohesive fracture modes. These findings are in line with previous literature on microhybrid composites and functional monomer-based adhesives, while contributing novel insights into the adhesive behavior of structurally distinct materials tested under identical experimental conditions.
CONCLUSIONS
Mechanical shear tests performed on the three composite materials used in the present study, including Charisma Classic (1_CH), G-ænial Anterior (2_GC) and Omnichroma (3_CA), yielded results that highlight clear differences in terms of adhesion to the tooth structure.
G-ænial Anterior (2_GC) presented the highest values of displacement strength and a cohesive fracture behavior, indicating a strong and stable adhesion, exceeding the internal resistance capacity of the composite. This type of mechanical response is considered ideal in direct restorations, suggesting good integration between the material and the tooth substrate. Its superior performance, both quantitatively and qualitatively, makes this material a recommended option in areas subject to intense functional stress.
Charisma Classic (1_CH) and Omnichroma (3_CA) recorded similar mean values of displacement force (~266–269 N), with a typical interfacial fracture behavior, without cracks in the composite mass. This type of displacement indicates a weaker, although constant, adhesion, requiring careful and correct application of the adhesive system to compensate for the mechanical limitations of the interface.
Thus, the overall conclusion of this study is that G-ænial Anterior provides a superior bond at the material–dental hard tissue interface compared to the other materials tested, which makes it particularly recommended for long-term direct restorations, especially in areas with high occlusal loading.
Data availability statement
The data supporting this study’s findings are available from the corresponding author upon reasonable request.
Acknowledgments
The authors would like to thank Assoc. Prof. PhD Mihai Cosmin Cotrut, Faculty of Materials Science and Engineering, National University of Science and Technology POLITEHNICA Bucharest, Romania, for the support and constructive comments.
We also gratefully acknowledge Mrs. Roxana Radvan from the National Institute for Research and Development in Optoelectronics (INOE), Bucharest, Romania, for her valuable insights and scientific support during the development of this work.
Conflicts of interest
None declared.
Financial support
None declared.
References
- 1.ZHAO Z, WANG Q, ZHAO J, et al. Adhesion of teeth. Frontiers in Materials. 2021;7:615225. [Google Scholar]
- 2.CARVALHO RM, MANSO AP, GERALDELI S, et al. Durability of bonds and clinical success of adhesive restorations. Dent Mater. 2012;28:72–86. doi: 10.1016/j.dental.2011.09.011. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 3.VAN MEERBEEK B, PEUMANS M, POITEVIN A, et al. Relationship between bond-strength tests and clinical outcomes. Dent Mater. 2010;26:e100–e121. doi: 10.1016/j.dental.2009.11.148. [DOI] [PubMed] [Google Scholar]
- 4.MUÑOZ MA, LUQUE-MARTINEZ I, MALAQUIAS P, et al. In vitro longevity of bonding properties of universal adhesives to dentin. Oper Dent. 2015;40:282–292. doi: 10.2341/14-055-L. [DOI] [PubMed] [Google Scholar]
- 5.YUAN X, WANG Q, HAN F, et al. Chemical interaction between 10-methacryloyloxydecyl dihydrogen phosphate and methacryloxypropyltrimethoxysilane in one-bottle dental primer and its effect on dentine bonding. J Mech Behav Biomed Mater. 2021;121:104610. doi: 10.1016/j.jmbbm.2021.104610. [DOI] [PubMed] [Google Scholar]
- 6.ISMAIL AM, BOURAUEL C, ELBANNA A, SALAH ELDIN T. Micro versus Macro Shear Bond Strength Testing of Dentin-Composite Interface Using Chisel and Wireloop Loading Techniques. Dent J (Basel) 2021;9:140. doi: 10.3390/dj9120140. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 7.CUEVAS-SUÁREZ CE, DA ROSA WLO, LUND RG, et al. Bonding Performance of Universal Adhesives: An Updated Systematic Review and Meta-Analysis. J Adhes Dent. 2019;21:7–26. doi: 10.3290/j.jad.a41975. [DOI] [PubMed] [Google Scholar]
- 8.KULZER GMBH. Charisma Classic: Light-curing universal composite. https://www.kulzer.com/en/en/products/charisma.html [Google Scholar]
- 9.GC CORPORATION. G-ænial Anterior & Posterior: Instructions for use. https://www.gc.dental/europe/sites/europe.gc.dental/files/products/downloads/gaenial/manual/MAN_G-aenial_Anterior-Posterior_en.pdf. 2011 [Google Scholar]
- 10.TOKUYAMA DENTAL AMERICA. Omnichroma: One-shade universal composite. https://www.tokuyama-us.com/omnichroma-dental-composite/ [Google Scholar]
- 11.HASSAN SHAYMAA. An Evaluation of Mechanical Properties of Different Types of Composite Resins (An in vitro Study) Al-Rafidain Dental Journal. 2014;14:123–131. [Google Scholar]
- 12.CHEN H, FENG S, JIN Y, et al. Comparison of bond strength of universal adhesives using different etching modes: A systematic review and meta-analysis. Dent Mater J. 2022;41:1–10. doi: 10.4012/dmj.2021-111. [DOI] [PubMed] [Google Scholar]
- 13.LAHARI AR, NAINAN MT, NIRUPAMA DN, et al. An in vitro study to compare shear bond strength of aged composite to two single-shade composites. J Conserv Dent Endod. 2024;27:1261–1266. doi: 10.4103/JCDE.JCDE_658_24. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 14.AZHEEN MOHAMAD MK, BESTOON MOHAMAD F. Effect of different surface treatments on repair bond strength of microhybrid and nanohybrid composite resins. Curr Trends Biomedical Eng Biosci. 2023;25:5556078. [Google Scholar]
- 15.JOHN JB, GAINNEOS PD, MATHEW BM, et al. Comparative evaluation of shear bond strength of two adhesive materials on demineralized dentin treated with silver diamine fluoride: An in-vitro study. Indian J Dent Res. 2021;32:395–398. doi: 10.4103/ijdr.ijdr_724_21. [DOI] [PubMed] [Google Scholar]
- 16.BINSALEH S, SULIMANY AM, ALDOWSARI MK, et al. Evaluation of the shear bond strength of a tricalcium silicate-based material to four self-adhering glass ionomer materials: an in vitro study. Frontiers in Pediatrics. 2023;11:1303005. doi: 10.3389/fped.2023.1303005. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 17.REN Z, WANG R, ZHU M. Comparative evaluation of bonding performance between universal and self-etch adhesives: in vitro study. Heliyon. 2024;10:e35226. doi: 10.1016/j.heliyon.2024.e35226. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 18.ELOLIMY GA, SHEBL EA. Artificial aging effect on color stability and bond strength of one-shaded versus multi-shaded composite resins. Tanta Dental Journal. 2024;21:419–427. [Google Scholar]
- 19.ALREFAI M, DEGIRMENCI A, PEHLIVAN IE. Shear bond strength of resin nanoceramic repairing with various single-shade resin composites. Essent Dent. 2023;35:101–107. [Google Scholar]
- 20.ARMSTRONG S, BRESCHI L, ÖZCAN M, et al. Academy of Dental Materials guidance on in vitro testing of dental composite bonding effectiveness to dentin/enamel using micro-tensile bond strength (μTBS) approach. Dental Materials. 2017;33:133–143. doi: 10.1016/j.dental.2016.11.015. [DOI] [PubMed] [Google Scholar]
Associated Data
This section collects any data citations, data availability statements, or supplementary materials included in this article.
Data Availability Statement
The data supporting this study’s findings are available from the corresponding author upon reasonable request.