Skip to main content
Scientific Reports logoLink to Scientific Reports
. 2026 Jan 6;16:3648. doi: 10.1038/s41598-025-33800-2

Multifunctional fast-curing polyaspartic ester polyurea/PANI-CsC@TiO2 composite coatings with antistatic and anticorrosion properties

Mirreza Gheybi 1, Abdolreza Mirmohseni 1,✉, Ali Olad 2
PMCID: PMC12848017  PMID: 41495128

Abstract

The growing requirement for multifunctional, fast-curing composite coatings has made polyaspartic ester polyurea (PAE-PU) systems more prominent in terms of their fast ambient curing and excellent mechanical and chemical properties. However, the combination of antistatic, antibacterial, and anticorrosion functionalities in PAE-PU coatings remains a significant challenge. In the present research work, a new multifunctional PAE-PU-based composite coating was developed and fabricated by incorporating a PANI-CsC@TiO2 composite. PANI-CsC@TiO2 composite was synthesized through in-situ polymerization of aniline onto glutaraldehyde-crosslinked chitosan-TiO2 (CsC@TiO2) matrix. Polyaspartic ester (PAE) resin prepared via a catalyst-free Michael addition reaction to achieve homogeneous molecular weight distribution (PDI: 1.034). Loading of the PANI-CsC@TiO2 composite into the PAE-PU matrix resulted in synergistic enhancement of antistatic, antibacterial, corrosion-resistant, and mechanical properties. At 2 wt%, surface resistivity dropped to 5.5 × 107 Ω/sq, and at 5 wt%, antibacterial activity rose significantly to 14 mm (S. aureus) and 9 mm (E. coli) inhibition zones. Corrosion current density decreased from 101 to 9 µA/cm2. This one-hour room-temperature-curing multifunctional coating shows promising potential as an alternative to standard epoxy and polyurethane systems under the tested conditions.

Supplementary Information

The online version contains supplementary material available at 10.1038/s41598-025-33800-2.

Keywords: Polyaspartic ester polyurea, Fast curing, Polyaniline, Chitosan, Antistatic, Anticorrosion

Subject terms: Chemistry, Materials science

Introduction

Chemical process equipment, as well as surface, operational, and recovery room equipment in hospitals, are continuously exposed to corrosive chemicals, microbial contamination, and electrostatic charge accumulation1. These factors can significantly reduce surface durability and equipment performance, accelerate corrosion, and compromise overall process safety2. Various methods have been reported to prevent these issues3,4. Among them, composite coatings have attracted researchers’ attention as advanced solutions for protecting surfaces and equipment5,6. Since composite coatings protect surfaces against various damaging factors, they play a vital role in maintaining surface integrity and extending their service life7–9. In the past decade, researchers have used polymeric coatings such as epoxy and polyurethane to develop composite coatings for surface protection10–13. For example, Li et al.14 prepared water-based polyurethane coatings with enhanced antibacterial and antistatic properties by dispersing a PANI/Cu/ZrO2 nanocomposite in a water-based polyurethane matrix. Mirmohseni et al.15 used PANI-CuZnO nanocomposites to create polyurethane coatings with antistatic and antibacterial properties. It was reported that the modified polyurethane coating had a surface resistance of 8⨯107 Ω /square. Despite advantages such as good adhesion to various substrates, suitable chemical resistance, and desirable flexibility, these coatings face specific challenges in the coating industry. One of the main challenges is their long curing time, which in some cases can range from several hours to several days, thereby reducing coating efficiency and the overall productivity of industrial operations16.

Two-component polyaspartic ester polyurea systems have increasingly attracted researchers’ attention in industrial protective applications, owing to their high mechanical strength, excellent wear resistance, and significantly shorter curing time compared to epoxy and polyurethane coatings9,17,18. The fast-curing capability of PAE-PU coatings makes them an ideal choice for fast, single-layer applications, offering a combination of desirable properties. These coatings contain ester groups adjacent to substituted amines, which, due to their ability to control reactivity, have resulted in a significant breakthrough in polyurea materials9. PAE resins, used in preparing PAE-PU coatings, are formed through the Michael addition reaction of primary amines with dialkyl maleates9,19. These resins can be synthesized without using any solvents and catalysts, following the tenets of one-step green synthesis, and are economically and environmentally friendly19–22. Owing to the favorable properties of PAE-PU coatings for surface protection, such coatings can be endowed with multifunctional additives to form composite coatings, and extend their application fields to chemical industries (protection against corrosion) and electronic industries (prevention against accumulation of electrostatic charge)3,23–26. Multifunctional additives, owing to their unique morphologies and surface properties, not only enhance the electrochemical and mechanical performances of polymer coatings, but also enhance the ability to prevent the growth of bacteria on polymer surfaces3,8. It should be emphasized that the performance of multifunctional coatings is strongly dependent on the homogeneous dispersion of nanocomposites in the polymer matrix. Poor dispersion can lead to aggregation, reduced effective interfacial area, and compromised performance. Recent studies have highlighted that incorporating well-dispersed multifunctional additives such as MXene-based hybrids, conductive polymer–inorganic frameworks, or organic–inorganic nanohybrids can dramatically improve the multifunctionality of polymer coatings27–29. Meng et al.30 prepared polyaspartic polyurea elastomers via the reaction of Desmophene NH1420 and isophorone diisocyanate (IPDI). The mechanical and thermal conductivity properties of the synthesized polyaspartic polyurea elastomers were improved through the incorporation of graphene nanoplates.

Polyaniline (PANI) is one of the most important conducting polymers due to the easy production and simple synthesis process31–35. PANI is used extensively in the creation of antistatic materials and corrosion-resistant coatings36. Unmodified PANI uses typically require a high loading in the polymer matrix to achieve the wished-for functional properties, compromising mechanical stability37. More recent investigations suggest that the addition of nanoparticles, i.e., ZnO and TiO2, to the PANI matrix increases conductivity and antibacterial properties but decreases the amount of PANI needed38–40. Such progress indicates that conducting polymer-TiO2 nanocomposites are an exciting way to enhance the functionality of PAE-PU coatings. It is worth noting that most prior studies have focused on incorporating PANI-based composites into epoxy or conventional polyurethane coatings. While such systems demonstrate useful antibacterial and antistatic properties, they generally suffer from long curing times, limited mechanical resilience, or lower compatibility with multifunctional fillers. In contrast, the use of a PAE-PU matrix offers unique advantages, including fast ambient curing, superior wear resistance, and eco-friendly synthesis. By introducing the PANI–CsC@TiO2 composite into the PAE-PU platform, this work combines the multifunctionality of the hybrid with the processing and performance benefits of PAE-PU. To the best of our knowledge, this is the first report of employing PANI–CsC@TiO2 in a PAE-PU system, thereby extending the application scope of conducting polymer–inorganic hybrids into next-generation protective coatings.

In this study, for the first time, a new multifunctional composite coating based on PAE-PU was developed, featuring enhanced antibacterial, antistatic, and anti-corrosion properties. The PAE resin was synthesized via a catalyst-free Michael addition reaction. CsC@TiO2 composite was synthesized through cross-linking chitosan by using glutaraldehyde, incorporating TiO2 nanoparticles, followed by in-situ polymerization of aniline to yield the PANI-CsC@TiO2 composite. Incorporating the composite into the resin matrix provided the formation of a multifunctional activity under the tested conditions. The composite coating prepared in this research boasts superior properties compared to standard systems, such as lower curing times, higher corrosion protection. Particularly, the achievement of such antistatic properties was facilitated by just 2 wt% of the PANI-CsC@TiO2 composite, which contrasts sharply with the general literature expectation that comparable levels of performance are achieved using higher concentrations of the additive. Such heightened efficacy, coupled with protective functionality and reduced curing times, highlights the potential application of the coating in advanced areas of the chemical and pharmaceutical industries, opening up avenues for the realization of the next-generation protective composite coatings.

Materials and methods

Materials

The commercial grade Maleic anhydride, Ethanol 96%, Toluene, Aliphatic polyisocyanate (DesmodurN75, 16.2%NCO content), Isophorone diamine (IPDA), Titanium Dioxide (TiO2 nanoparticles) was provided by Oshim Shimi Company, Sanyar, Isfahan Petrochemical Co, BASF, Essen and Covestro companies respectively. Glutaraldehyde (GA, Extra Pure, 50% Solution) and Chitosan (Cs, low molecular weight) were purchased from Sigma Aldrich and used as received. Hydrochloric acid (HCL, 37%), N-Methyl-2-pyrrolidone (NMP, 99.5%), Ammonium persulfate (APS, 98%), and Aniline (99.8%) were acquired from Merck Co. Notably, Aniline was double-distilled before use.

Synthesis of DEM

The synthesis was carried out by an esterification reaction using maleic anhydride, as shown in Fig. 2a, according to standard procedures41,42. A round-bottom flask, provided with a thermometer, reflux condenser, and Dean-Stark apparatus, was used, to which were added maleic anhydride (48.44 g, 0.8 mol) and ethanol (147.42 g, 3.2 mol). Thorough homogenizing was carried out, to which sulfuric acid (11.3 g) was then added dropwise under incessant mixing. To facilitate the extraction of the water formed as a by-product in the reaction, toluene (15 mL) was added as a medium for the transport of water, successfully reducing the azeotropic point of the mixture of water and ethanol and improving the efficiency in the elimination of water. A temperature range of 80 to 90 °C was sustained for 3.5 h to ensure effective esterification process completion. Upon reaction completion, the product formed was neutralized using the 10% sodium carbonate (pH = 7) to remove any remaining sulfuric acid and unreacted components. The product was then dried over anhydrous sodium sulfate, while toluene was evaporated by distillation below boiling point.

Fig. 2.

Fig. 2

Synthesis schematic for DEM (a) and CsC@TiO2 composite (b).

Preparation of PAE resin

PAE resin was synthesized by a Michael addition reaction9,19. In a 250 mL three-neck round-bottom flask equipped with a nitrogen inlet, reflux condenser, and magnetic stirrer, one mole of IPDA was charged at room temperature. Two moles of DEM were added dropwise over a period of 1 h at 35–40 °C. The temperature was increased to 80–85 °C, and the reaction was left under nitrogen for 24 h. The synthetic pathway to DEM and PAE resin is illustrated in Figs. 1a, b.

Fig. 1.

Fig. 1

Synthesis pathway of DEM (a) and PAE resin (b). FTIR spectra of DEM and PAE resin (c).

Synthesis of cross-linked chitosan@TiO2 composite

2.5 g of Cs was dissolved in 100 mL of 1% acetic acid solution and stirred. Then, 20 mL of 0.025 M GA was added and stirred for 15 h. 1 g of TiO2 nanoparticles was gradually added to the mixture, stirring for 5 more hours. The solution was then mixed with 0.5 M NaOH solution, and after the formation of a precipitate, the solid product was filtered, washed with deionized water, and dried at 80 °C (Fig. 2b)43.

Synthesis of PANI and PANI- CsC@TiO2 composite

0, 5, and 10 wt% CsC@TiO2 composites were dissolved in 125 mL of 1.7 M HCl and stirred for 1 h. 10 g of aniline was added followed by addition of 22.8 g ammonium persulfate (APS) in 125 mL of 1.7 M HCl and added dropwise within 2 h at -5 °C. The reaction was continued for 4 h under the same temperature. The precipitate was washed with HCl, filtered, and dried at 60 °C for 12 h. The products were designated as PANI, PANI 1, and PANI 2 for 0, 5, and 10 wt% CsC@TiO2, respectively. To convert PANI from the emeraldine salt form to emeraldine base, 3 g of PANI and PANI 2 were soaked in ammonia solution (500 ml, 0.1 M, 3 h) and dried at 65 °C for 12 h.

Preparation of PAE-PU/ PANI-CsC@TiO2 composite coatings

Different amounts of de-doped PANI-CsC@TiO2 (0, 1, 2, 3, and 5 wt%) were mixed with PAE resin dissolved in NMP solvent. Then, 2.35 g of hardener (Desmodur N75) was added and mixed. The mixture was applied to a substrate and cured for 24 h. After curing, the film was doped in a dilute HCl solution (1.7 M) for 5 h, washed with deionized water, and dried at 25 °C for 24 h. The prepared composite films are listed in Table 1.

Table 1.

PAE -PU composites coatings with different PANI-CsC@TiO2 contents.

Composite films PAE resin
(g)
NMP
(g)
PANI-CsC@TiO2
(wt%)
Desmodur N75
(g)
PAE 2.5 0.25 0 2.35
PAE 1 2.5 0.25 1 2.35
PAE 2 2.5 0.25 2 2.35
PAE 3 2.5 0.25 3 2.35
PAE 4 2.5 0.25 5 2.35

Characterization

Characterization techniques included FTIR (Bruker Tensor 27, Germany) for DEM, PAE resin, CsC@TiO2, PANI, and PANI-CsC@TiO2, FESEM and EDX (MIRA 3 TESCAN, Czech Republic) for morphological and elemental analysis, and the surface roughness was assessed by AFM (Nanosurf Mobile S, Switzerland). The XRD (Bruker D8 ADVANCE, Germany) for structural analysis of PANI, CsC@TiO2, and PANI-CsC@TiO2 in the 2θ range of 10°–60°. Molecular weight distribution of PAE resin was determined by GPC (KNAUER, Germany). Mechanical performance was evaluated by tensile test (ASTM D638, Al-7000 M GOTECH, Taiwan), adhesion strength (ASTM D4541, ERICHSEN 525), and hardness/scratch resistance (ISO 1518, TQC Pen Hardness Tester). The water contact angle has been measured with CAG-10 instrument (Iran). Further details on characterization procedures, such as amine value measurement, electrical conductivity, antistatic properties, antibacterial tests, electrochemical measurements, and calculations involved, are available in supporting information.

Results and discussion

Characterization of PAE-PU-based coatings

The curing behavior

The amine values of IPDA and PAE resin were 660 mg KOH/g and 193.9 mg KOH/g, respectively (Table 2). The decrease in the amine value of PAE resin is attributed to the reaction between the primary amines of IPDA and the C = C groups of DEM19. Using Eq. (3) (supporting information), it was calculated that 94 g of isocyanate is required to cure 100 g of PAE resin with an amine equivalent weight of 289.32 g/mol and an NCO/NH ratio of 1.05.

Table 2.

Amine value and amine equivalent weight for IPDA and PAE resin.

Samples Amine value (mg KOH/g) Amine equivalent weight (g/mol)
IPDA 660 85
PAE resin 193.9 289.32

The curing behaviour of the pure PAE coating and PAE coatings with 1, 2, 3, and 5 weight% PANI-CsC@TiO2 composite is shown in Table 3. The findings show that the curing parameters are not significantly altered by the addition of the composite. All formulations show virtually the same gelation and final curing profiles, suggesting that the composite only serves as a physical reinforcement within the polymer matrix and does not chemically participate in the curing reactions44.

Table 3.

Curing behavior of the pure PAE-PU coating and PAE-PU coatings incorporating varying loadings of PANI–CsC@TiO2 composite.

Samples PANI-CsC@TiO2 (wt%) Pot life (min) Gel time (min) Curing time (min)
PAE 0 8 16 57
PAE 1 1 8 16 57
PAE 2 2 8 16 57
PAE 3 3 8 16 57
PAE 4 5 8 16 57

Comparative curing behavior of PAE-PU coating with reference to conventional polyurea and epoxy coatings was conducted (Table 4). The PAE-PU coating possessed a gel time of 16 min, which was significantly higher than polyurea (3 s). This longer gel time is attributed to steric hindrance by the secondary amine structure, which inhibits reaction with isocyanates and takes more time, providing more application time. On the other hand, polyurea resins are quick to cure due to the reactive isocyanates and primary amines that lead to quick curing, which is difficult to control45.

Table 4.

Comparison of curing behavior of different polymeric resins.

Resin – Curing agents Pot life (min) Gel time (min) Curing time (min) Ref
Polyurea- PMDI - 0.05 10–25 46
Epoxy/ TETA 45 105 230 47
PAE - Desmodur N75 8 16 57 This work

GPC analysis of PAE resin

Gel permeation chromatography (GPC) was conducted to assess the molecular weight distribution and homogeneity of the PAE resin (Fig 3). The number average molecular weight (Mn) and weight average molecular weight (Mw) were found to be 1869 Da and 1934 Da, respectively, with a polydispersity index (PDI) of 1.035. These results confirm that the PAE resin was synthesized successfully, resulting in a homogeneous structure with a narrow molecular weight distribution48.

Fig. 3.

Fig. 3

GPC chromatogram of PAE resin.

FTIR analysis

Fourier transform infrared spectroscopy (FTIR) was utilized to examine and compare the spectral features of the synthesized DEM and PAE resin, as shown in Fig. 1c. The peak observed at 1642 cm− 1 is attributed to the C = C bond in diethyl maleate. This peak diminishes upon reaction with the NH2 groups of primary diamines and disappears completely when all double bonds have reacted in spectrum of PAE resin, a stretching vibration at 3339.7 cm− 1 is related to N-H groups of secondary amin. The peak at 2950.42 cm− 1 is attributed to the stretching vibrations of aliphatic C-H bonds. The stretching vibration of C = O bonds and the bending vibration of C-N bonds are proved by the bands at 1732.62 cm− 1 and 1170.18 cm− 1, respectively49. Also, the peak at 1028.80 cm− 1 corresponds to the C-O-C stretching vibration. All the mentioned peaks provide evidence for the reaction between DEM and IPDA19.

Characterization of the PANI and PANI-CsC@TiO2 composites

Structural analysis by FTIR

FTIR spectra of TiO2 nanoparticles, chitosan (Cs), CsC@TiO2, PANI, and PANI-CsC@TiO2 composite are presented in Fig. 4a. The TiO2 spectrum shows a peak at 721 cm-1 ascribed to Ti-O-Ti vibration50. The chitosan spectrum shows peaks at 3453 cm-1 and 2864.18 cm-1, ascribed to O-H and N-H stretching and C-H stretching, respectively51. The FT-IR spectrum of CsC@TiO2 composite is identical to that of its components. In addition, the peaks for the -NHCO vibration at 1646 and 1379 cm-1 are characteristic of the presence of an amide, formed by the introduction of TiO2 into the crosslinked chitosan using glutaraldehyde43. In the PANI spectrum, the stretching vibrations of the C=C and C=N bonds of the benzenoid and quinoid rings appear at 1464 cm-1 and 1559 cm-1 respectively. The peak at 1114 cm-1 confirms the quinoid units of the PANI chain. The C-H bonds of benzenoid ring are shown at 794 cm-1 and 701 cm-1. Also, two peaks at 2857 cm-1 and 2924 cm-1 are related to the stretching vibrations of the aromatic ring’s C-H bonds. The FTIR spectrum of the PANI-CsC@TiO2 composite displays all the peaks of PANI, although some of them are observed at lower wavenumbers compared to pure PANI. This shift may be attributed to physicochemical interactions, such as hydrogen bonding between PANI and Cs or TiO2. Specifically, the interaction between TiO2 and PANI appears to weaken the Ti-O bond. The O-H and N-H stretching peaks of the PANI-CsC@TiO2 composite have shifted from 3435.02 cm-1 to 3432.7 cm-1, suggesting possible hydrogen bonding interactions between PANI and CsC@TiO2, as inferred from peak shifts. While these spectral changes are consistent with hydrogen bonding reported in similar systems, direct confirmation would require further analyses (e.g., FTIR deconvolution, NMR)23.

Fig. 4.

Fig. 4

FTIR spectra of TiO2, Chitosan, CsC@TiO2, PANI, and PANI-CsC@TiO2 (a) and XRD patterns of CsC@TiO2, PANI, and PANI-CsC@TiO2 (b).

Analysis of XRD

XRD patterns for PANI, CsC@TiO2, and the PANI-CsC@TiO2 composite are presented in Fig. 4b. The XRD pattern of the CsC@TiO2 composite displays two broad and prominent peaks at approximately 2θ = 12.14° and 20.14°. These peaks are indicative of chitosan’s presence and align with values documented in the literature. This unique fingerprint pattern is commonly observed in semi-crystalline chitosan materials, which is attributed to their amorphous polymeric nature. The existence of TiO2 in the composite is demonstrated by the peaks observed at 2θ = 25.32°, 27.46°, 38.27°, and 47.9°, which align well with the standard diffraction data (JCPDS 21-1272 and 21-1276)52,53. These peaks verify that the crystalline TiO2 phase remains intact within the nanocomposite. The observed peaks of PANI at 20.68˚, 14.50˚, and 25.36˚ (corresponding to the 020, 011, and 200 lattice planes) are linked to the partially crystalline nature of PANI chains (emeraldine salt)54. The combination of distinct peaks of PANI and CsC@TiO2 is visible in the PANI-CsC@TiO2 composite.

Morphological studies and EDX analysis

Figure 5 illustrates the morphologies of pure PANI, CsC@TiO2, and the PANI-CsC@TiO2 composite. The pure PANI in aggregate form is revealed in Fig. 5a. Uniformly distributed on the chitosan surface are the TiO2 nanoparticles of average particle diameter 36.24 nm (Figs. 5b, c). This uniform distribution contributes to an enhanced effective surface area of chitosan. The low and high magnification FESEM images of the PANI-CsC@TiO2 composite, which contains 10 wt% CsC@TiO2, are presented in Figs. 5d, e. The similarity in morphology between PANI-CsC@TiO2 and the unmodified CsC@TiO2 composite indicates that the PANI component likely created a thin, conformal coating or shell around the CsC@TiO2 composite during the in-situ polymerization process. To confirm the presence of TiO2 in both the CsC@TiO2 composite and the PANI-CsC@TiO2 composite, energy-dispersive X-ray (EDX) spectroscopy was employed (Figs. 5f, g, h). The PANI-CsC@TiO2 composite shows a TiO2 content of 7.02 wt%, which implies that the addition of TiO2 significantly improves the electrical conductivity of the composite compared to pure PANI.

Fig. 5.

Fig. 5

FESEM micrographs and EDX spectra of PANI (a, f), CsC@TiO2 (b, c, f), and PANI-CsC@TiO2 (d, e, h).

Study of electrical conductivity

The electrical conductivity of pure PANI and the PANI-CsC@TiO2 composite was assessed at room temperature (298 K) using the four-point probe technique. Table 5 displays the recorded electrical conductivity values for pure PANI and its corresponding composites. The addition of various percentages of CsC@TiO2 significantly improves the conductivity of PANI. This enhancement may be linked to a decrease in the conjugated chain length of PANI as the amount of TiO2 nanoparticles increases. Such a reduction in chain length could result from strong interactions between the PANI chains and TiO2 nanoparticles. A possible explanation is the interaction between TiO2 and PANI chains, which may facilitate charge transfer, as suggested in previous studies. However, confirming this mechanism would require advanced studies such as DFT calculations or charge transfer spectroscopy23,54. The composite with 10% CsC@TiO2 was selected for further investigation due to its superior electrical conductivity.

Table 5.

Electrical conductivity values of PANI and PANI-CsC@TiO2 composites containing various percentages of CsC@TiO2.

Samples Electrical properties
CsC@TiO2 (wt%) Conductivity (S cm− 1)
PANI 0 0.98 ± 0.2
PANI 1 5 3.10 ± 0.1
PANI 2 10 5.40 ± 0.2

Evaluation of composite coatings based on PAE-PU

FTIR analysis of pure and PAE-PU composite coatings

FTIR spectra of the pure PAE coating and of the samples incorporating 1, 3, and 5 wt% of the PANI–CsC@TiO2 composite are shown in Fig. 6. Pure PAE coating FTIR spectrum revealed a wide, intense band at 3418 cm− 1 according to N–H stretching of the urea functional group and possible O–H stretching, verifying the extensive hydrogen-bonding network of the polyurea backbone. Methylene C–H stretches appeared at 2923 and 2853 cm− 1, and ester and hydrogen-bonded urea carbonyls were evident at 1704 and 1634 cm− 1, respectively55. Other bands at 1540 cm⁻¹ (amide II), 1460 cm− 1 (C–H bending), 1163–1024 cm− 1 (C–O–C stretching), and 763 cm− 1 (out-of-plane N–H bending) cumulatively contributed to the unique polyaspartic polyurea framework19,30. Introduction of PANI–CsC@TiO2 composite (1–5 wt%) produced severe spectral changes, suggesting physicochemical interactions between the different existing functional groups of additives and resin components. In the 3200–3600 cm− 1 region, the large N–H/O–H band shape and intensity changed, and a shoulder at 3423–3425 cm− 1 in the 3 and 5 wt% samples, attributed to free N–H or O–H groups of chitosan and partial disruption of the polymer hydrogen-bonding network. New peaks in 1500–1700 cm− 1 region at 1518 cm− 1 (benzenoid C–C stretching of PANI) and 1655 cm− 1 (C = C/C = N stretching in quinonoid rings of PANI or Schiff-base groups of chitosan) also confirmed the existence of PANI. Meanwhile, ester and urea carbonyl bands shifted slightly, intensity changed, or became deformed, consistent with hydrogen-bond formation between the polymer C = O groups and N–H/O–H groups of the composite56,57.

Fig. 6.

Fig. 6

FTIR spectra of the pure PAE coating and its composite coatings containing 1, 3, and 5 wt% PANI–CsC@TiO2.

SEM and AFM surface morphology analysis of the composite coatings

The FESEM micrographs depicted in Fig. 7a and b correspond to the unmodified PAE-PU coating and the coating incorporating 5 wt% PANI-CsC@TiO2 after HCl doping, respectively. The FESEM and AFM images of the other samples (1, 2, and 3 wt% composites) are provided in the Supporting Information (Fig. S1). As one can observe in Fig. 7a, the pristine coating surface is very smooth and uniform, with no apparent microstructural features. This indicates a homogeneous polymeric matrix with no apparent nanostructural inclusions. On the contrary, Fig. 7b indicates a much more ordered, rough surface texture with clear morphological features. These are the outcome of effective incorporation and dispersion of the PANI-CsC@TiO2 composite in the polymeric matrix, which alters the surface topology and introduces heterogeneity. This change in morphology is also supported by the three-dimensional AFM images (Fig. 7c and d). The surface of the neat PAE-PU coating (Fig. 7c) is quite flat, without considerable surface roughness and small peak-to-valley height features, indicating a smooth topography. However, AFM of the modified coating (Fig. 7d) indicates a very high surface roughness, with more apparent topographical features and greater protrusions. The Z-axis height profile shows a substantial increase in vertical surface variation, as predicted, with the addition of the PANI-CsC@TiO2 composite followed by acid doping introducing an enhanced and heterogeneous surface morphology. This higher surface roughness may successfully enhance interfacial interactions to result in improved functional properties such as barrier performance, hydrophilicity, or antibacterial activity.

Fig. 7.

Fig. 7

FESEM images of the pure PAE-PU coating (a) and the PAE-PU coating modified with 5 wt% PANI-CsC@TiO2 composites after HCl doping (b). AFM images of the pure PAE-PU coating (c) and the modified PAE-PU coating with 5 wt% PANI-CsC@TiO2 composites after HCl doping (d).

Figure 8 demonstrates elemental mapping and EDS analysis of the HCl-doped PAE-PU coating with 5 wt% PANI-CsC@TiO2 composites. For the coatings incorporating 1, 2, and 3 wt% of the composite, the corresponding EDS spectra and elemental mapping results are provided in the Supporting Information (Figs. S2–S4). Homogeneous distribution of Cl, O, N, C, and Ti on the surface of the coating ensures effective incorporation and fine dispersion of composite components within the polymer matrix58. PANI and the chitosan chains supply the majority of the carbon, nitrogen, and oxygen, while titanium shows that TiO2 was properly inserted into the final structure. Chlorine is also seen as a result of PANI being doped with HCl during assembly, which improves PANI’s structural stability and electrical conductivity in the finished coating. According to the homogeneous elemental mapping shown in Fig. 8. Such homogenous distribution is critical for reproducibility of electrical, mechanical, and anticorrosion properties, in agreement with recent research where effective dispersion of multifunctional nanofillers was indicated as the most relevant factor to enhance performance28,59.

Fig. 8.

Fig. 8

FESEM image, EDS spectrum, and elemental mapping of the PAE-PU coating modified with 5 wt% PANI-CsC@TiO2 composites after HCl doping.

Antistatic property

The surface electrical resistivity of PAE-PU coatings was analysed with varying amounts of pure PANI and PANI-CsC@TiO2 composites. The results of the surface resistivity measurements (Tables 6 and 7, and Fig. 9a) clearly show that incorporation of PANI–CsC@TiO2 into the PAE–PU matrix significantly improves the antistatic properties of the coatings. While the pristine PAE–PU coating exhibited a resistivity in the insulating regime (1013 Ω/sq), addition of even 2 wt% PANI–CsC@TiO2 reduced the surface resistivity to 5.5 × 107 Ω/sq, in the normal antistatic window (105–109 Ω/sq). This is consistent with previous reports, i.e., epoxy/PANI–Cs–TiO2 coatings with 3.7 × 107 Ω/sq at identical loading. Thus, it illustrates that the synergistic effect of TiO2 and cross-linked chitosan significantly enhances dispersion and enables conductive networks to be established at low concentration levels compared to pure PANI54.

Table 6.

The surface resistivity of the PAE-PU coating with PANI and PANI-CsC@TiO2 additive.

Samples Surface resistivity (109Ω /sq)
0 1Wt% 2 Wt% 3 Wt% 5 Wt%
PAE-PU/PANI composite coatings 1013 0.2282 ± 0.001 0.1171 ± 0.002 0.0440 ± 0.001 0.0250 ± 0.003
PAE-PU/PANI-CsC@TiO2 composite coatings 1013 0.1013 ± 0.002 0.0550 ± 0.001 0.0281 ± 0.002 0.0001 ± 0.001

Table 7.

A comparison of the antistatic properties of PAE-PU coatings with other coatings.

Resin Additive Quantity (%) Surface resistivity (Ω sq− 1) Ref.
Polyaspartic ester polyurea PANI-CsC@TiO2 2 5.5⨯107 This work
Epoxy PANI-Chitosan-TiO2 2 3.7⨯107 54
Waterborne Polyurethane P-Cu@ZnO 2 1.2⨯108 60
Waterborne epoxy PANI-SiO2 30 6.6⨯1010 61

Fig. 9.

Fig. 9

Surface resistivity of PAE-PU coatings containing various percentages of PANI and PANI-CsC@TiO2 composite (a). Water contact angle measurements of PAE-PU-based coatings (b).

Comparisons with other polymeric systems (Table 7) further serve to highlight the increased efficiency of the present formulation: whereas waterborne epoxy/PANI–SiO2 required as much as 30 wt% of filler to achieve the antistatic range, the PAE–PU/PANI–CsC@TiO2 system was able to accomplish this performance with just 2 wt%. The steep drop in resistivity from 1 to 2 wt% is an indication that the percolation point lies around 2 wt%, where continuous pathways of conductance are established. The increase of the filler content to 5 wt% decreased the resistivity even further (1 × 105 Ω/sq), though less than with 2 wt%, further ensuring that electrical conductivity is susceptible to plateauing once the percolation threshold has been reached.

It must be realized that the composite loading was not increased beyond 5 wt%. Higher filler loadings are typically associated with particle agglomeration, poor interfacial compatibility, and microstructural heterogeneity, which not only may inhibit further conductivity gain but may even deteriorate coating uniformity. Also, overloading with hard fillers can weaken the mechanical properties of the coating through increased brittleness and reduced adhesion strength, also found in corresponding studies on PANI- and metal oxide-based nanocomposites. Therefore, maintaining the loading in the range 2–5 wt% offers a good balance of conductivity, dispersion stability, and mechanical performance.

Investigation of water contact angle (WCA) of the PAE-PU composite coatings

WCA measurements (Table 8; Fig. 9b) are significant to provide information regarding the barrier performance and wettability of coatings62,63. The neat PAE–PU coating had a very low WCA value of 46.39°, indicating a highly hydrophilic surface prone to water permeation and ionic mobility. Increase of just 1 wt% PANI–CsC@TiO2 brought the WCA to 58.46°, which means that even minimum amounts of the hybrid composite impart noticeable surface heterogeneity and incomplete hydrophobicity due to the presence of the PANI chains and TiO2 domains. With the continued addition of the composite, the WCA continuously increased to 65.32° at 3 wt% and to 72.57° at 5 wt%. This regular increase in hydrophobicity is due to the synergistic effect of PANI and TiO2: PANI provides a more compact molecular structure on the coating surface, while TiO2 nanoparticles generate micro/nanoscale roughness, both reducing the effective surface energy64,65. Also, the presence of crosslinked chitosan facilitates structural integrity and inhibits excess swelling, thus further enhancing water repellency. It is important to realize that before HCl doping, hydrophobicity is regulated by morphological heterogeneity rather than protonation of PANI. The stepwise WCA increase with increased filler loading verifies that increased filler loads enable better surface roughness and coverage, which prevent direct water adsorption. The effect is best at 5 wt%, where additional amounts can realistically lead to particle agglomeration and loss of homogeneity. Finally, the progressive increase in WCA from 46.39° (0 wt%) to 72.57° (5 wt%) before doping unmistakably demonstrates that incorporation of PANI–CsC@TiO2 significantly increases the barrier properties of the PAE–PU coatings by reducing surface wettability and water absorption pathways, hence being beneficial in improving their long-term corrosion protection. After HCl doping, WCA of the PAE–PU/PANI–CsC@TiO2 films enhanced progressively from the undoped state. At 1 wt% loading, it enhanced from 58.46° to 63.92°, at 3 wt% from 65.32° to 73.09°, and at 5 wt% from 72.57° to 84.09°. This enhancement is mainly ascribed to protonation of the PANI backbones, giving rise to conformational rearrangements and a denser surface structure with reduced surface energy66,67. In addition, the doped films exhibited higher nanoscale roughness and more uniform distribution of Cl dopant ions, both contributing to reduced wettability. Generally, HCl doping significantly improved the hydrophobicity and barrier properties of the films, justifying their improved corrosion protection.

Table 8.

The WCA of the different coating before and after doping by immersion in HCl in the presence PANI-CsC@TiO2.

Samples 0 1% 3% 5%
Pure PAE-PU 46.39 ± 0.2 - - -
PAE-PU with PANI-CsC@TiO2 before doping - 58.46 ± 0.28 65.32 ± 0.31 72.57 ± 0.32
PAE-PU with PANI-CsC@TiO2 after doping - 63.92 ± 0.11 73.09 ± 0.18 84.09 ± 0.21

Antibacterial properties

Gram-positive and Gram-negative bacteria were used to test the coatings’ antibacterial qualities. Antibacterial testing (Table 9; Fig. 10) confirmed that pure PAE-PU coating did not show any detectable inhibition against S. aureus or E. coli, while incorporating 5 wt% PANI-CsC@TiO2 resulted in potent antibacterial activity with 14 mm and 9 mm inhibition zones, respectively. The enhanced activity is a result of synergistic interaction among PANI, TiO2, and crosslinked chitosan68. Protonated PANI transfers cationic charges, which electrostatically interact with negatively charged bacterial membranes, leading to cell wall damage and leakage of intracellular components. TiO2 nanoparticles also promote antibacterial activity through the generation of reactive oxygen species (ROS), which induce oxidative stress and structural damage in bacterial cells70–73. Additionally, crosslinking chitosan with glutaraldehyde increases its rigidity and structural strength with increased availability of amino groups for bacterial interaction74.

Table 9.

The effect of addition of different percentage of PANI-CsC@TiO2 into the PAE-PU on Inhibition zone of S. aureus and E. coli.

PAE-PU composite coatings with PANI-CsC@TiO2 (wt%) Inhibition zone (mm)
S. aureus E. coli
0% 0 0
1% 0 0
3% 8 ± 0.5 5 ± 0.4
5% 14 ± 0.6 9 ± 0.3

Fig. 10.

Fig. 10

Antibacterial activity of PAE-PU coatings with PANI and PANI-CsC@TiO2 composite against S. aureus and E. coli (a). Inhibition zone diameters for PAE-PU coatings with PANI and PANI-CsC@TiO2 composite against E. coli and S. aureus (b).

The coating showed greater inhibition of Gram-positive S. aureus compared to Gram-negative E. coli, consistent with reports that the outer lipopolysaccharide layer of Gram-negative bacteria provides a diffusion barrier against the entry of ROS and cationic polymers68. Interestingly, up to 5 wt% of PANI-CsC@TiO₂ was utilized in the present study. This optimal concentration was selected on the basis of two main reasons: (1) the antibacterial activity showed a sharp increase above 3 wt% and reached a plateau at 5 wt%, i.e., further loadings would not proportionally enhance the activity due to saturation of the bacterium surface ; (2) over-inclusion of conducting polymers is also known to cause aggregation and impair mechanical properties and coating adhesion. Indeed, it has already been demonstrated in epoxy and polyurethane systems that PANI loadings above ~ 7–10 wt% cause phase segregation and loss of flexibility15,54. Therefore, the 5 wt% level is a point at which antibacterial activity, antistatic activity, and mechanical integrity are all optimized together.

Mechanical properties

Figure 11 present the adhesion strength and scratch resistance of pure and modified polyaspartic ester coatings containing 1, 3, and 5 wt% PANI-CsC@TiO2 composite. The effectiveness and durability of coatings are significantly influenced by its adhesion to the underlying substrate. Consequently, the study examined how the addition of PANI-CsC@TiO2 composite affects the adhesion strength of polyaspartic ester polyurea coatings to concrete substrates. Results from the Pull off test indicate that the adhesive strength of the coatings increases with a higher content of composite (Fig. 11a). This improvement in adhesion may be associated with possible interfacial interactions, including coordination of titanium ions (TiO2) with surface oxygen atoms of concrete, and potential hydrogen bonding between amino groups of PANI and hydroxyl groups of the substrate. While these mechanisms are consistent with previous reports, they are proposed here as plausible explanations rather than definitive proof, since direct spectroscopic or surface energy measurements were not performed75,76.

Fig. 11.

Fig. 11

Effect of PANI-CsC@TiO2 composite content on (a) adhesion strength and (b) scratch resistance of PAE-PU-based coatings.

Another important factor affecting the functionality and appearance of the coatings is scratch resistance. the scratch resistance data of the developed polyaspartic ester polyurea coatings revealed that increasing nanocomposite content leads to improved scratch resistance (Fig. 11b). This enhancement is likely related to interactions between polymer chains and TiO2 nanoparticles that may compact the chains and improve load transfer. However, this interpretation remains hypothetical and would require further verification (e.g., DMA or nanoindentation) to confirm the exact mechanism54.

Table 10 shows that the tensile strength of the unmodified resin (0.877 MPa) went up when the composite was added. The composite increased the Young’s modulus (from 4.94 to 10.23 MPa), but decreased the elongation at break. These changes suggest that interfacial interactions (such as possible hydrogen bonding and chain packing effects) reduced chain mobility and increased stiffness. Nevertheless, these results should be interpreted cautiously, as more advanced characterization (DMA, FTIR deconvolution) would be required to directly confirm such mechanisms.

Table 10.

The mechanical properties of coatings made of pure PAE-PU and PAE-PU composite .

Samples Young’s modulus
(MPa)
Tensile strength
(MPa)
Elongation at break
(%)
PAE 4.94 ± 0.2 0.877 ± 0.1 28.94 ± 1
PAE 1 5.99 ± 0.4 0.929 ± 0.3 25.01 ± 1
PAE 3 8.35 ± 0.2 0.971 ± 0.3 23.34 ± 0.5
PAE 4 10.23 ± 0.5 1.171 ± 0.2 24.40 ± 1

Evaluation of corrosion resistance

To evaluate the corrosion protective performance of pristine PAE-PU coatings (PAE) and its formulation reinforced with 5 wt% of the PANI-CsC@TiO2 composite (PAE 4), polarization tests and electrochemical impedance spectroscopy (EIS) were conducted after 24 h of immersion in 1 M HCl solution. This acidic medium was deliberately chosen to represent a highly aggressive corrosive environment relevant to chemical industries. However, it should be noted that other corrosive media such as saline (NaCl) and alkaline solutions were not examined in this work. Future studies will extend the evaluation to these environments to provide a more comprehensive understanding of the coating’s anticorrosion performance. The results are presented in Fig. 12; Tables 11 and 12.

Fig. 12.

Fig. 12

Tafel plots (a) and Nyquist plots (b) for bare mild steel, PAE, and PAE 4 samples in HCl solution (1 M), with equivalent circuit models for (c) bare and (d) coated samples.

Table 11.

Potentiodynamic polarization results for bare mild steel, PAE, and PAE-4 samples.

samples Ecorr
(mV)
Icorr
(µA/cm2)
Ba
(V/dec)
Bc
(V/dec)
Rp
(Ω cm2)
Bare -500 149 0.084 0.068 109
PAE -507 101 0.091 0.100 206
PAE 4 -543 9 0.119 0.159 3046

Table 12.

EIS parameters of the bare substrate (mild steel), PAE, and PAE 4 samples.

Samples CPE-coat R coat
(Ω.cm2)
CPE-dl R ct
(Ω.cm2)
Fitting error
Y0 × 10− 6
(Ω−1cm−2Sn)
n 1 Y0 × 10− 6
(Ω−1cm−2Sn)
n 2
bare - - - 178.16 0.91 32 0.0003
PAE 148.74 0.86 181 159.19 0.70 22 0.0009
PAE 4 10.06 0.67 2789 0.52 0.85 34 0.0007

The Tafel plots (Fig. 12a) show that the corrosion potential (Ecorr) was more negative in the PAE 4 sample (-543 mV) than in the uncoated steel (-500 mV) and the neat PAE-PU coating (-507 mV). This means that the cathodic protection was better77. The corrosion current density (Icorr) in the PAE 4 sample dropped a lot to 9 µA/cm2, which is much lower than the neat PAE coating (101 µA/cm2) and the uncoated sample (149 µA/cm2).

The increase in polarization resistance (Rp) in the PAE 4 sample to 3046 Ω cm2 indicates a significant enhancement in surface electrochemical resistance, which is due to the formation of a dense, uniform, and highly inhibitive protective layer. Similar improvements in corrosion resistance have been reported in systems where engineered interfacial or layered microstructures effectively block aggressive species and suppress charge transfer, underscoring the critical role of interface design in corrosion protection78,79. The presence of the PANI-CsC@TiO2 composite plays a key role in this improvement. On the one hand, PANI, due to its p-type semiconducting nature, can form a passive layer on the metal surface and limits electron exchange80. On the other hand, TiO2, which its n-type semiconducting behavior, reduces electric charge transfer and, by creating composite structures, effictively blocks the penetration of aggressive ions81. The crosslinked Cs also contribute by creating a cohesive network that improves adhesion to the substrate and prevents the spread of corrosion by filling micro-defects82.

The EIS results (Fig. 12b), especially the Nyquist plot analysis, show that the arc diameter for the PAE 4 sample is much bigger, which means that it has more charge transfer resistance (Rct)83,84. Table 12 shows that Rct for PAE 4 was 34 Ω cm2, which is higher than the 22 Ω cm2 for neatPAE and the 32 Ω cm2 for uncoated steel. This means that PAE 4 is more resistant to corrosion. Also, the coating resistance (Rcoat) went up a lot, from 181 Ω cm2 in neat PAE to 2789 Ω cm2 in PAE 4. This shows that the modified composite structure is better at protecting itself. Analogously, recent studies in electrochemical systems have demonstrated that engineered interlayers can regulate ion diffusion and suppress interfacial charge transfer, thereby significantly enhancing interfacial stability85.

The equivalent circuits used for EIS data analysis (Figs. 12c, d), consisting of solution resistance (Rs), Rcoat, Rct and two constant phase elements (CPE), provided a very good fit (error ≤ 0.01), confirming excellent agreement of the experimental data with the theoretical model.

Electrochemical analysis and modeling show that adding PANI-CsC@TiO2 makes the PAE-PU coating much better at preventing corrosion. This improvement is due to things like making the surface rougher, making it stick better, and making it less permeable. These changes suggest that the coating has promising potential for use in acidic and corrosive environments under the tested laboratory conditions.

It should be noted, however, that the present work was particularly focused on demonstrating the multifunctionality of the coatings synthesized (antistatic, antibacterial, anticorrosion, and mechanical strengthening). There was no detailed examination of the environmental impact (humidity or temperature), nor durability under longer-term tests (UV aging, thermal cycling, or abrason resistance after extended periods). Both are of utmost relevance for applied utilization and are principal lines of future investigation.

Conclusion

This study successfully designed and synthesized a multifunctional fast-curing PAE-PU composite coating for use in surface protection applications. Antistatic, antibacterial, mechanical, and anti-corrosion properties were significantly enhanced by the addition of the engineered PANI-CsC@TiO2 composite to the polymer matrix. The PAE resin had a narrow molecular weight distribution (PDI: 1.035) and was produced using a catalyst-free method. The coating with 2 wt% of the composite worked well as an antistatic coating, with a surface resistivity of 5.5 × 107 Ω/sq. It was very effective at killing bacteria at a concentration of 5 wt%, with inhibition zones of 14 mm against S. aureus and 9 mm against E. coli. The corrosion current density dropped by more than 90%, but the polarization resistance shot up to 3046 Ω cm2. Also, the coating’s adhesion strength, scratch resistance, and Young’s modulus were all improved without hurting its structural integrity. The PAE-PU/PANI-CsC@TiO2 composite coating demonstrated significant multifunctional improvements under the tested conditions, suggesting its potential as a promising protective coating for industrial and biomedical applications.

Supplementary Information

Below is the link to the electronic supplementary material.

Supplementary Material 1 (5.2MB, docx)

Acknowledgements

The authors are grateful to the University of Tabriz for providing support for this research.

Author contributions

All authors have contributed equally in the preparation of manuscript. All authors have reviewed the manuscript.

Funding

No funding.

Data availability

All data generated or analysed during this study are included in this published article [and its supplementary information files].

Declarations

Competing interests

The authors declare no competing interests.

Footnotes

Publisher’s note

Springer Nature remains neutral with regard to jurisdictional claims in published maps and institutional affiliations.

References

  • 1.Zhang, P. et al. Investigation on aging behavior and failure mechanism of blast-resistant polyurea coating in service environments. Mater. Today Commun.44, 112051 (2025). [Google Scholar]
  • 2.Zhu, D., Hu, S., Fu, Y., Zhao, N. & Liu, D. A review of Preparation methods, friction and wear, corrosion, and biocompatibility of biomedical high-entropy alloys. J. Mater. Sci.59, 1153–1183 (2024). [Google Scholar]
  • 3.Naeini, P. S., Dorraji, M. S. S., Rastgar, M., Azizi, M. & Daei, F. The role of zinc molybdate in the anticorrosion and antibacterial characteristics of sustainable polyurethane coating derived from epoxidized soybean oil. Ind. Crops Prod.216, 118771 (2024). [Google Scholar]
  • 4.Liu, X. et al. First-principles analysis of effects of cerium doping on electrochemical corrosion behaviors of steel. J. Rare Earths. 43, 1758–1768 (2025). [Google Scholar]
  • 5.Zhao, Y., Jing, J., Chen, L., Xu, F. & Hou, H. Current research status of interface of ceramic-metal laminated composite material for armor protection. Acta Met. Sin. 57, 1107–1125 (2021). [Google Scholar]
  • 6.Shokri Asri, D., Aber, S., Teimuri-Mofrad, R. & Rezaei, A. Robust porous Fe,Co-Nc cathode catalyst derived from SiO2-Protected Ferrocene-ZIF-67 for enhanced microbial fuel cell performance. Energy Fuels. 39, 23662–23674 (2025). [Google Scholar]
  • 7.Haddadi, S. A. et al. Zinc-doped silica/polyaniline core/shell nanoparticles towards corrosion protection epoxy nanocomposite coatings. Compos. Part. B Eng.212, 108713 (2021). [Google Scholar]
  • 8.Mirmohseni, A., Azizi, M. & Dorraji, M. S. S. Cationic graphene oxide nanosheets intercalated with polyaniline nanofibers: A promising candidate for simultaneous anticorrosion, antistatic, and antibacterial applications. Prog Org. Coat.139, 105419 (2020). [Google Scholar]
  • 9.Natour, S. et al. Aspartate-based polyurea coatings: ambient cure process and inevitable transformation of Urea groups into hydantoin cycles in polyurea networks and their impact on film properties. Prog Org. Coat.192, 108449 (2024). [Google Scholar]
  • 10.Liu, Y., Meng, F., Wang, F. & Liu, L. Dual-action epoxy coating with anti-corrosion and antibacterial properties based on well-dispersed ZnO/basalt composite. Compos. Commun.42, 101674 (2023). [Google Scholar]
  • 11.Islam, M. et al. Rheological and antimicrobial properties of epoxy-based hybrid nanocoatings. Polym. Test.81, 106202 (2020). [Google Scholar]
  • 12.Sun, L. et al. Fabrication of an anti-fouling coating based on epoxy resin with a double antibacterial effect via an in situ polymerization strategy. Prog Org. Coat.184, 107837 (2023). [Google Scholar]
  • 13.Gao, F. et al. Preparation of graphene oxide-based polyaniline composites with synergistic anticorrosion effect for waterborne polyurethane anticorrosive coatings. Prog Org. Coat.156, 106233 (2021). [Google Scholar]
  • 14.Li, X., Xu, X. & Zhang, F. Antistatic and antibacterial two-component waterborne polyurethane coating. J. Coat. Technol. Res.20, 869–881 (2023). [Google Scholar]
  • 15.Mirmohseni, A., Rastgar, M. & Olad, A. Preparation of PANI–CuZnO ternary nanocomposite and investigation of its effects on polyurethane coatings antibacterial, antistatic, and mechanical properties. J. Nanostructure Chem.8, 473–481 (2018). [Google Scholar]
  • 16.Li, Q., Weinell, C. E. & Kiil, S. Curing-induced internal stress in epoxy coatings: effects of epoxy binder, curing agent, filler, initial solvent concentration, curing temperature, and relative humidity. Prog Org. Coat.173, 107175 (2022). [Google Scholar]
  • 17.Wang, H. et al. Silicone-modified polyurea-interpenetrating polymer network fouling release coatings with excellent wear resistance property tailored to regulations. J. Colloid Interface Sci.653, 971–980 (2024). [DOI] [PubMed] [Google Scholar]
  • 18.Park, J. et al. Synthesis and properties of eco-friendly coatings using waterborne polyaspartic and blocked isocyanate. Mol. Cryst. Liq Cryst.688, 1–6 (2019). [Google Scholar]
  • 19.Dural, S. & Camadanlı, S. Ş. Kayaman Apohan, N. Improving the mechanical, thermal and surface properties of polyaspartic ester bio-based polyurea coatings by incorporating silica and Titania. Mater. Today Commun.38, 107654 (2024). [Google Scholar]
  • 20.Maksó, L. et al. Catalyst-and excess reagent recycling in aza-Michael additions. Org. Biomol. Chem.22, 2465–2473 (2024). [DOI] [PubMed] [Google Scholar]
  • 21.Trampuž, M., Stavber, G. & Likozar, B. Catalyst-free aza-Michael addition for C–N coupling in active pharmaceutical ingredient synthesis: modelling of thermodynamic, reaction kinetics and mass transfer considerations. Chem. Eng. J.374, 924–936 (2019). [Google Scholar]
  • 22.Zhang, Y. et al. Bagasse-based porous flower-like MoS2/carbon composites for efficient microwave absorption. Carbon Lett.35, 145–160 (2025). [Google Scholar]
  • 23.Mirmohseni, A., Rastgar, M. & Olad, A. Effectiveness of PANI/Cu/TiO2 ternary nanocomposite on antibacterial and antistatic behaviors in polyurethane coatings. J. Appl. Polym. Sci.137, 48825 (2020). [Google Scholar]
  • 24.Xavier, J. R., Bhaskar, R. & Subramanian, S. Multifunctional graphitic carbon nitride/manganese dioxide/epoxy nanocomposite coating on steel for enhanced anticorrosion, flame retardant, mechanical, and hydrophobic properties. J. Ind. Eng. Chem.134, 514–536 (2024). [Google Scholar]
  • 25.Gao, X. et al. When it’s heavier: interfacial and solvation chemistry of isotopes in aqueous electrolytes for Zn-ion batteries. Angew Chem. Int. Ed.62, e202300608 (2023). [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 26.Han, K. et al. Self-healing and antistatic waterborne polyurethane hybrid coating resulting from hard but reversible Zr-O-Si networks. Chem. Eng. J.487, 150538 (2024). [Google Scholar]
  • 27.Du, P., Wang, J., Hsu, Y. I. & Uyama, H. Homogenous organohydrogel mediated by Covalently-Converted graphene nanosheets as an electronic epidermis for multimodal perception and soft actuation. ACS Mater. Lett.6, 2974–2984 (2024). [Google Scholar]
  • 28.Yadav, V., Pal, D. & Poonia, A. K. Nanofillers as a potential key for shaping the future of the industries. Hybrid. Adv.7, 100340 (2024). [Google Scholar]
  • 29.Guo, D. et al. Interaction of nanostructured Lu2Si2O7/Lu2SiO5 double-ceramic layer environmental barrier coatings with CMAS. Surf. Coat. Technol.502, 131994 (2025). [Google Scholar]
  • 30.Meng, Q. et al. Polyaspartic polyurea/graphene nanocomposites for multifunctionality: Self-healing, mechanical resilience, electrical and thermal conductivities, and resistance to corrosion and impact. Thin-Walled Struct.189, 110853 (2023). [Google Scholar]
  • 31.Goswami, R. N. et al. Polyaniline-wrapped h-boron nitride nanosheets as anticorrosive filler in epoxy coatings for substantially enhanced protection of mild steel. J. Ind. Eng. Chem.140, 285–297 (2024). [Google Scholar]
  • 32.Beygisangchin, M. et al. Recent progress in polyaniline and its composites; Synthesis, properties, and applications. Eur. Polym. J.11294810.1016/j.eurpolymj.2024.112948 (2024).
  • 33.Wen, J. et al. Recent progress in polyaniline-based chemiresistive flexible gas sensors: design, nanostructures, and composite materials. J. Mater. Chem. A. 10.1039/D3TA07687C (2024). [Google Scholar]
  • 34.Caldas, C. M., Calheiros, L. F. & Soares, G. Silica–polyaniline hybrid materials prepared by inverse emulsion polymerization for epoxy-based anticorrosive coating. J. Appl. Polym. Sci.134, 45505 (2017). [Google Scholar]
  • 35.Wang, J. et al. Ultrasensitive electrochemical detection of tumor cells based on multiple layer cds quantum dots-functionalized polystyrene microspheres and graphene oxide–polyaniline composite. Biosens. Bioelectron.100, 1–7 (2018). [DOI] [PubMed] [Google Scholar]
  • 36.Rangel-Olivares, F., Arce-Estrada, E. & Cabrera-Sierra, R. Development of polyaniline/chitosan (PANI/CTS) and TiO2-PANI/CTS nanocomposites as anti-corrosion coatings: synthesis and characterization. Surf. Coat. Technol.476, 130163 (2024). [Google Scholar]
  • 37.Liu, B. T., Syu, J. R. & Wang, D. H. Conductive polyurethane composites containing polyaniline-coated nano-silica. J. Colloid Interface Sci.393, 138–142 (2013). [DOI] [PubMed] [Google Scholar]
  • 38.Al-Masoud, M. A., Khalaf, M. M., Mohamed, I. M., Shalabi, K. & Abd El-Lateef, H. M. Computational, kinetic, and electrochemical studies of polyaniline functionalized ZnO and ZnO-SiO2 nanoparticles as corrosion protection films on carbon steel in acidic sodium chloride solutions. J. Ind. Eng. Chem.112, 398–422 (2022). [Google Scholar]
  • 39.Zhang, H. et al. Polyaniline/ZnO heterostructure-based ammonia sensor self-powered by electrospinning of PTFE-PVDF/MXene piezo-tribo hybrid nanogenerator. Chem. Eng. J.496, 154226 (2024). [Google Scholar]
  • 40.Alamgeer et al. Polyaniline/ZnO hybrid nanocomposite: Morphology, spectroscopy and optimization of ZnO concentration for photovoltaic applications. Polymers15, 363 (2023). [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 41.Bhagiyalakshmi, M., Priya, S. V., Mabel, J. H., Palanichamy, M. & Murugesan, V. Effect of hydrophobic and hydrophilic properties of solid acid catalysts on the esterification of maleic anhydride with ethanol. Catal. Commun.9, 2007–2012 (2008). [Google Scholar]
  • 42.Xuehui, L., Zhenping, C., Yingwen, L., Jinxing, L. & Lefu, W. Method for Preparing maleate by selective catalytic oxidation of lignin. US Pat. NO : 10807938B2, (2020).
  • 43.Billah, R. E. K. et al. Adsorptive removal of cr (VI) by chitosan-SiO2-TiO2 nanocomposite. Environ. Nanotechnol Monit. Manag. 18, 100695 (2022). [Google Scholar]
  • 44.Bhadra, J., Alkareem, A. & Al-Thani, N. A review of advances in the Preparation and application of polyaniline based thermoset blends and composites. J. Polym. Res.27, 122 (2020). [Google Scholar]
  • 45.Squiller, E. P. et al. Polyaspartic coating compositions US Pat NO: 9944821B2 (2018).
  • 46.Sendijarevic, V. et al. Hydrolytic stability of toluene diisocyanate and polymeric Methylenediphenyl diisocyanate based polyureas under environmental conditions. Environ. Sci. Technol.38, 1066–1072 (2004). [DOI] [PubMed] [Google Scholar]
  • 47.Mirmohseni, A. & Pourtaghi-Zahed, H. Polyamidoamines based on castor oil‐styrene co‐oligomer/triethylenetetramine as curing agents in high‐performance epoxy coatings. J. Appl. Polym. Sci.137, 49082 (2020). [Google Scholar]
  • 48.Jiang, S. et al. Highly branched polyurea-enhanced urea-formaldehyde resin. ACS Appl. Polym. Mater.3, 1157–1170 (2021). [Google Scholar]
  • 49.Wang, J., Zhang, J., Cheng, G., Zhang, K. & Liu, X. Performance and mechanism of Tetracycline removal by peroxymonosulfate-assisted double Z-scheme LaFeO3/g-C3N4/ZnO heterojunction under visible light drive. Environ. Technol. Innov.39, 104302 (2025). [Google Scholar]
  • 50.Perumal, G. Production of biodiesel from waste cooking oil using a novel surface-functionalized CaMoO4/ TiO2 solid catalyst. Renew. Energy. 228, 120652 (2024). [Google Scholar]
  • 51.Guo, Z. et al. Co-pyrolysis and co-combustion characteristics of low-rank coal and waste biomass: insights into interactions, kinetics and synergistic effects. J. Energy Inst.118, 101918 (2025). [Google Scholar]
  • 52.Hussein, E. M., Desoky, W. M., Hanafy, M. F. & Guirguis, O. W. Effect of TiO2 nanoparticles on the structural configurations and thermal, mechanical, and optical properties of chitosan/TiO2 nanoparticle composites. J. Phys. Chem. Solids. 152, 109983 (2021). [Google Scholar]
  • 53.Matakgane, M., Mokoena, T. P., Kroon, R. E., Mofokeng, S. J. & Mhlongo, M. R. Robust upconversion luminescence of Ho3+/Yb3 + co-doped TiO2 nanophosphors manifested by crystallinity. J. Mol. Struct.1305, 137747 (2024). [Google Scholar]
  • 54.Mirmohseni, A., Rastgar, M. & Olad, A. PANI-chitosan‐TiO2 ternary nanocomposite and its effectiveness on antibacterial and antistatic behavior of epoxy coating. J. Appl. Polym. Sci.136, 47629 (2019). [Google Scholar]
  • 55.Cheng, S., Han, Z., Zhao, H., Li, Y. & Lu, S. A novel bifunctional Pt/Ce/WZrOx catalyst for efficient selective oxidation of high-concentration NH3. Chem. Eng. J.479, 147876 (2024). [Google Scholar]
  • 56.Rezaei, A., Aber, S., Asghari, E. & Elmas, S. Tailoring macro-microporous carbon using porphyrin-based zeolitic imidazole framework as an efficient cathodic component for microbial fuel cell. Fuel374, 132508 (2024). [Google Scholar]
  • 57.Sun, Q. et al. Microstructural evolution and kinetics of monoclinic scheelite-type BiVO4-based materials with enhanced color performance. Ceram. Int.51, 40414–40430 (2025). [Google Scholar]
  • 58.Baishya, H., Dutta, J. & Kumar, S. Nanofillers reinforcing biopolymer composites for sustainable food packaging applications: A State-of‐the‐Art review. Adv Funct. Mater 2503819 (2025).
  • 59.Li, Y. et al. A Biomass-Derived Imine-Linked waterborne polyurethane for Self-Healable anticorrosive coating. ACS Appl. Polym. Mater.10.1021/acsapm.5c02428 (2025).41164357 [Google Scholar]
  • 60.Mirmohseni, A., Azizi, M. & Seyed Dorraji, M. S. A promising ternary nanohybrid of Copper@ zinc oxide intercalated with polyaniline for simultaneous antistatic and antibacterial applications. J. Coat. Technol. Res.16, 1411–1422 (2019). [Google Scholar]
  • 61.Nguyen, A. S. et al. Synthesis of conducting PANi/SiO2 nanocomposites and their effect on electrical and mechanical properties of antistatic waterborne epoxy coating. J. Coat. Technol. Res.17, 361–370 (2020). [Google Scholar]
  • 62.Moone, L. et al. Tunable wettability of phenolic resin coatings. Prog Org. Coat.198, 108883 (2025). [Google Scholar]
  • 63.Chang, J. et al. Surface topography effects on the wettability and antifouling performance of nano-ZnO epoxy composite coatings. Surf. Coat. Technol.433, 128145 (2022). [Google Scholar]
  • 64.Li, M. et al. Photothermal and hydrophobic surfaces with Nano-Micro structure: fabrication and their Anti-Icing properties. Nanomaterials15, 378 (2025). [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 65.Hu, C., Kwan, K., Xie, X., Zhou, C. & Ren, K. Superhydrophobic polyaniline/TiO2 composite coating with enhanced anticorrosion function. React. Funct. Polym.179, 105381 (2022). [Google Scholar]
  • 66.Li, Z. & Gong, L. Research progress on applications of polyaniline (PANI) for electrochemical energy storage and conversion. Materials13, 548 (2020). [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 67.Liao, G., Li, Q. & Xu, Z. The chemical modification of polyaniline with enhanced properties: A review. Prog Org. Coat.126, 35–43 (2019). [Google Scholar]
  • 68.Muñoz-Bonilla, A. & Fernández-García, M. Polymeric materials with antimicrobial activity. 372 Top. Issue Biomater.37, 281–339 (2012). [Google Scholar]
  • 69.Zhang, J. et al. Impact of reactive oxygen species on cell activity and structural integrity of Gram-positive and Gram-negative bacteria in electrochemical disinfection system. Chem. Eng. J.451, 138879 (2023). [Google Scholar]
  • 70.Varghese, M. & Balachandran, M. Antibacterial efficiency of carbon Dots against Gram-positive and Gram-negative bacteria: A review. J. Environ. Chem. Eng.9, 106821 (2021). [Google Scholar]
  • 71.Maruthapandi, M., Saravanan, A., Gupta, A., Luong, J. H. & Gedanken, A. Antimicrobial activities of conducting polymers and their composites. Macromol2, 78–99 (2022). [Google Scholar]
  • 72.Tikhonov, V. E. et al. Bactericidal and antifungal activities of a low molecular weight Chitosan and its N-/2(3)-(. Carbohydr. Polym.64, 66–72 (2006). [Google Scholar]
  • 73.Athanasoulia, I. G., Mikropoulou, M., Karapati, S., Tarantili, P. & Trapalis, C. Study of thermomechanical and antibacterial properties of TiO2/Poly(lactic acid) nanocomposites. 11th Panhellenic Sci. Conf. Chem. Eng. (2017).
  • 74.Yeh, Y. et al. The role of Aldehyde-Functionalized crosslinkers on the property of Chitosan hydrogels. Macromol. Biosci.22, 2100477 (2022). [DOI] [PubMed] [Google Scholar]
  • 75.Ashassi-Sorkhabi, H., Moradi-Alavian, S., Jafari, R., Kazempour, A. & Asghari, E. Effect of amino acids and montmorillonite nanoparticles on improving the corrosion protection characteristics of hybrid sol-gel coating applied on AZ91 Mg alloy. Mater. Chem. Phys.225, 298–308 (2019). [Google Scholar]
  • 76.Wang, L. et al. Investigation on the effects of polyaniline/lignin composites on the performance of waterborne polyurethane coating for protecting cement-based materials. J. Build. Eng.64, 105665 (2023). [Google Scholar]
  • 77.Liu, Y. et al. Tribocorrosion behaviours and mechanisms of inconel 625–nano/micro Al2O3 composite coatings prepared by plasma enhanced high-velocity Arc spraying. Corros. Sci.256, 113221 (2025). [Google Scholar]
  • 78.Ling, Z. et al. Enhanced corrosion resistance of laser-remelted Fe–Cr–B–Mo alloy through interfacial periodic layered structures in liquid aluminum. J. Mater. Res. Technol.37, 4717–4731 (2025). [Google Scholar]
  • 79.Ling, Z., Yang, W., Chen, W. & Fu, Z. Recent advances in Understanding the corrosive effects of molten aluminum on structural materials and protective strategies: A comprehensive review. Mater. Today Commun.47, 113249 (2025). [Google Scholar]
  • 80.Olad, A. & Nosrati, R. Preparation and corrosion resistance of nanostructured PVC/ZnO–polyaniline hybrid coating. Prog Org. Coat.76, 113–118 (2013). [Google Scholar]
  • 81.Cui, H. et al. Recent progress of ultrasound-responsive titanium dioxide sonosensitizers in cancer treatment. Chin. Chem. Lett.35, 109727 (2024). [Google Scholar]
  • 82.Li, Y., Yang, S. & Wan, Y. Hydroxyapatite-reinforced Chitosan film on PEO-treated aluminum alloys for enhanced corrosion resistance. J. Mater. Res. Technol.36, 5911–5924 (2025). [Google Scholar]
  • 83.WANG, X. et al. Defect-engineered rGO – CoNi2S4 with enhanced electrochemical performance for asymmetric supercapacitor. Trans. Nonferrous Met. Soc. China. 35, 563–578 (2025). [Google Scholar]
  • 84.Zhao, W. et al. Multiobjective-Optimization MoS2/Cd-ZnIn2S4/CdS composites prepared by in situ Structure-Tailored technique for High-Efficiency hydrogen generation. Small Struct.5, 2300569 (2024). [Google Scholar]
  • 85.Hu, Z. et al. In situ integration of rapid Ion-Diffusion interlayers on Cu current collectors toward ultrafast Anode-Free sodium metal batteries. ACS Nano. 19, 23193–23208 (2025). [DOI] [PubMed] [Google Scholar]

Associated Data

This section collects any data citations, data availability statements, or supplementary materials included in this article.

Supplementary Materials

Supplementary Material 1 (5.2MB, docx)

Data Availability Statement

All data generated or analysed during this study are included in this published article [and its supplementary information files].


Articles from Scientific Reports are provided here courtesy of Nature Publishing Group

RESOURCES