Abstract
In many existing brick buildings, severe dampness of the walls is often observed. One of the most common causes of severe dampness is a lack of adequate damp-proofing and frequent flooding. The strong capillary water absorption capacity causes that in some cases, brick masonry reaches the full water saturation state. Strong moisture has a negative impact on the mechanical parameters of brick masonry. However, the scale of this effect in brick buildings is an issue that is still largely unknown. In this paper, results of research conducted on brick, mortars, and masonry specimens are presented. The material specimens were cut out from a historic military building and tested in air-dry and wet conditions. Studies have shown that strong moisture significantly reduces compressive strength in all the tested materials. The reduction in compressive strength of the brick masonry ranged from 6% to 39%. Based on experimental results, this paper proposes a method for predicting the reduction in compressive strength of brick masonry caused by significant moisture. This method is based on testing specimens of brick and mortar taken from the structure and can be classified as a minor-destructive technique. Therefore, it can be particularly useful in assessing the sensitivity to the effects of significant moisture in historic structures, where the collection of larger masonry specimens for testing is not permitted due to conservation reasons.
Keywords: Brick masonry, Strong moisture, Compressive strength, Modulus of elasticity
Subject terms: Engineering, Materials science, Natural hazards
Introduction
For many centuries, bricks made from fired clay were the primary material used to construct buildings. There is a common problem with severe dampness of the walls in brick buildings erected in the past1–3. The presence of strong moisture in masonry walls can have many causes. The most common cause of strong moisture is capillary water rising from the soil. In ceramic brick walls, the process of capillary water rising is very intensive4–6. In buildings without damp-proofing, water is drawn up through capillaries in masonry materials, even to a height of several metres above ground level. Increased wall dampness in brick buildings can also be caused by flooding of the walls with rainwater, condensation of water vapor, and wet construction processes that may occur during renovation or reconstruction of historic buildings. Exceptional situations related to flooding of brick walls during floods are unfavorable from a structural point of view. Progressive climate change causes floods to occur increasingly. As a result, situations of flooding of walls of the lowest stories and sudden capillary water rise to higher storeys are becoming more frequent. The state of full water saturation of masonry walls due to floods can last for many weeks or even months, because in very thick masonry walls the process of surface drying is very slow7,8.
The effects of strong moisture on masonry walls include limitations in the use of buildings, the development of dangerous organisms on the surface of walls, crystallization of salts in the pores of masonry materials, defects in bricks and mortar caused by frost processes, and changes in the mechanical parameters of masonry. In analyses of the load-bearing capacity of walls and pillars, the change in strength and deformability of brick masonry under compression due to strong moisture is particularly important.
The effect of the influence of strong moisture on masonry’s strength was not provided in the code for masonry structures EN 1996-1-19. EN 1052-110 provides a laboratory method for determining the compressive strength of masonry. The method recommended by EN 1052-110 for seasoning test specimens indicates that the obtained compressive strengths of masonry refer to the air-dry condition. However, this code does not provide the method for seasoning masonry specimens to the wet condition or testing masonry in such a condition.
Research on brick masonry in different states of dampness was carried out by Bouška et al.11. The research was inspired by the great flood that occurred in the Czech Republic in 1997. Brick columns with dimensions of 450 × 450 × 1400 mm were made in the laboratory using lime mortar. The compressive strength of the masonry in the wet state was found to be 29% lower than the strength of the masonry in the air-dry state. Tests also recorded an increase in transverse deformations of masonry under compression caused by strong moisture.
A.M. Amde et al.12 investigated brick masonry prisms made using cement and cement-lime mortar. Lower compressive strength of the prisms in the wet condition was obtained in comparison to the compressive strength of the prisms in the air-dry condition. For prisms with cement mortar, the reduction was 14%, while for prisms with cement-lime mortar, it was 20%.
Extensive studies of the compressive strength of masonry in various moisture conditions were conducted by J. Witzany et al.13. Brick columns with a cross-section of 450 × 450 mm were made using lime mortars. The moisture contents of the tested columns were 1.36%, 3.56%, 14.26%, and 15.81%. The highest compressive strength, 3.1 MPa, was obtained for columns in the air-dry condition (with a moisture content of 3.56%), while the lowest compressive strength, 1.88 MPa, was characteristic of columns in the wet condition (with a moisture content of 15.81%). The strength decreased by 40%. The studies conducted by Witzany et al.13 also showed the effect of strong moisture in masonry on their increased deformability under compression.
Masonry made from low-strength materials was studied by T. Martins et al.14. The materials used in the studies were identical to those used to construct buildings in Portuguese cities in the 19th and 20th centuries. The state of full water saturation was obtained by immersing the masonry in water tanks. The compressive strength of the masonry in the wet condition was 15% lower than the strength of the masonry in the air-dry condition.
The decrease in the compressive strength of brick masonry due to their strong moisture was also observed in the research conducted by N. Sathiparan and U. Rumeshkumar15. The studies were conducted on masonry prisms consisting of 3 brick layers. Three types of mortar were used to make the prisms. The reduction in the compressive strength of the prisms caused by strong moisture ranged from 8% to 24%.
The prism made of high-strength bricks and mortars in the wet condition was studied by E. Franzoni et al.16. Bricks with a compressive strength of over 37 MPa and mortar with a strength of 19 MPa are usually not found in historic buildings. The test results presented in16 can rather be referred to structures built at present. The tests achieved a 6% reduction in the compressive strength of the masonry in the wet condition compared to the strength of the masonry in the air-dry condition.
The masonry built of modern bricks with low water absorption was also studied by D.V. Bompa and Y.A. Eighazani17. The masonry prisms consisting of 5 layers of bricks and joints were made from lime mortar, and then half of them were immersed in water to 3/5 of their height. The remaining layers of the masonry were subjected to capillary absorption. The compressive strength of the masonry in the air-dry condition was 4.28 MPa, while in the wet condition it was 4.24 MPa. The observed decrease in the compressive strength of the masonry was therefore minimal. However, in these studies, a 12% decrease in the value of the modulus of elasticity of the masonry in the wet condition was noted.
The studies conducted so far show that the mechanical parameters of brick masonry in the wet condition are worse than those in the air-dry condition. The decrease in the compressive strength of masonry in the wet condition ranged from a few to 40%, depending on the type of materials used. It should be emphasized that the studies conducted so far concerned masonry made in the laboratory from bricks and mortars produced today. Historic masonry are characterized by different properties. This results from the fact that different technologies for manufacturing masonry materials and constructing masonry structures were used in the past. The properties of historic bricks were mainly influenced, apart from the type of material used for their production, by the method of their manual forming and firing in small traditional charcoal kilns. On the other hand, the properties of the mortar in the joints were determined by the composition of the mortar, including primarily the type of binder, aggregate, and various types of organic and inorganic additives used, which are not used in mortars today18–20. A characteristic feature of the masonry materials used in the past for constructing buildings was their low strength and high porosity. The quality of workmanship on many historic masonry structures was also low, which is why many damages are recorded in buildings, such as cracks, deformations, and local crumbling of masonry materials21,22. The result of significant and continuous cracking of the masonry structure is seen in its division into separate fragments. This can ultimately lead to the collapse of the building. This masonry failure mechanism is often observed in cases of localized overloading of the structure or uneven settlement due to the deformations of building foundations23,24.
The question therefore arises as to what extent the relations obtained from tests on brick masonry specimens carried out on specimens made in laboratories from contemporary materials can be applied to historic masonry.
For this reason, a research program was developed, using original historic materials. The tests presented in this paper were carried out on masonry columns cut out of a building erected at the end of the 19th century. The masonry specimens were cut out of the building walls during its reconstruction with the conservator’s consent. Some of the masonry columns were tested in the air-dry condition, while some were tested in the wet condition (fully saturated with water). Specimens of bricks and mortar taken from the historic structure were also tested in the air-dry and the wet condition.
Based on the test results, the minor-destructive method was proposed for assessing the reduction in compressive strength of masonry due to strong moisture, based on tests of brick and mortar specimens taken from existing structures. This method should be considered as a preliminary solution for assessing the impact of strong moisture on the strength and deformability of masonry structures.
Compressive tests
The specimens for testing were taken from a building erected at the end of the 19th century. In the past, the building was used as a warehouse for cannons and ammunition (Fig. 1a).
Fig. 1.
View of the historical building (a), extraction of masonry columns using circular saw (b), method of protecting the masonry samples against damage (c).
The building’s structure was made of fired ceramic bricks. At the beginning of the 21st century, a decision was made to reconstruct the facility and change its function. During the renovation, some of the interior walls and sections of the exterior masonry walls were demolished. From the fragments of structures intended for demolition, masonry columns for strength tests were cut out using a diamond circular saw (Fig. 1b). At least two columns were cut from each wall. After cutting, the groups of columns were marked as C1, C2, C3, and C4. To avoid damage during transport to the laboratory, the columns were secured with plastic wrap and tape (Fig. 1c). The columns had cross-sections of 290 × 290 mm and a height of 5 to 7 masonry layers (Fig. 2).
Fig. 2.
Masonry columns collected from historical building.
Bricks and fragments of bed joints were also taken from the masonry walls from which the columns were cut out. The bricks were taken whole, thoroughly cleaned of any remaining mortar, and measured. The dimensions of the bricks were 283 × 135 × 65 mm (length x width x height).
The mortar for testing was taken from the bed joints using a metal chisel. The specimens taken from the joints had irregular shapes, which were then formatted (Fig. 3).
Fig. 3.
Preparation of mortar specimens.
Masonry columns, bricks and mortars were seasoned for at least 6 months at a temperature of 20 °C ± 2 °C and relative humidity 65% ± 3%.
After 6 months, cuboidal specimens of bricks and mortars were prepared. Each brick was cut into two halves. One half of the brick was designated for testing in the air-dry condition, and the other half in the wet condition. The brick specimens were aligned with a thin layer of cement mortar with a cement-sand ratio of 1:1. The flatness and parallelism of the surfaces through which the load was to be applied were in accordance with the EN 772-125.
The mortar specimens with cross-sections of 50 mm x 50 mm were formatted using the diamond saw. The height of mortar specimens was equal to the thickness of the joint. The dimensions of the mortar specimens were in accordance with DIN 18555-926. Two specimens were prepared from the same fragment of bed joint – one for testing in the air-dry condition and the other for testing in the wet condition. Since the mortar specimens did not have even surfaces, caps made of quick-setting cement mortar were used. The caps were prepared using steel punches with a diameter of 30 mm.
The specimens prepared for testing in the air-dry condition were stored in the laboratory at a temperature of 20 °C ± 2 °C and relative humidity of 65% ± 3%.
The brick and mortar specimens for tests in the wet state were first placed with their bases in cold water to enable capillary action to take place. Then, the specimens were completely immersed in water for 7 days.
For masonry columns, two wet seasoning methods were used. The first method, marked as “seasoning method A”, included a capillary rise phase followed by full immersion in water for 7 days (Fig. 4a). In the second method, marked as “seasoning method B”, after the capillary rise phase, the columns were clad with wet mats and protected against drying out by wrapping them with plastic foil (Fig. 4b). Each day of conditioning, the mats were soaked in water.
Fig. 4.
Methods of seasoning the brick columns to the wet condition. (a) “method seasoning A”, (b) “method seasoning B”.
Bricks were tested according to EN 772-125 (Fig. 5a). The compressive strength of the brick (fB) was calculated as the ratio of the maximum force to the surface area of the specimen.
Fig. 5.
Compressive strength tests (a) brick, (b) mortar, (c) masonry column.
For mortar specimens, the procedure given in DIN 18555-926 was used. This method, known as the double punch test (DPT), is used to test mortar specimens cut from the joints of the masonry walls. The steel punches had a diameter of 20 mm. Mortar specimens were placed between the punches and subjected to compression (Fig. 5b). Mortar compressive strength in the double punch test (fDPT) was defined as the ratio of the ultimate force to the surface area of the steel punch. The heights of the mortar samples (t) were equal to the thickness of the bed joints from which they were cut, and differed significantly. For this reason, the test results were recalculated using the relationship given in27.
![]() |
1 |
where: fDPT – mortar compressive strength obtained from DPT test, t – height of mortar specimen, d – diameter of steel punch.
The masonry column undergoing strength tests is shown in Fig. 5c. The deformations of masonry columns were measured using LVDT sensors. Compressive loads were applied such that the tests lasted from 15 to 30 min. At subsequent load levels, crack development and crumblings of bricks and mortars in joints were registered. After completing the strength tests, small brick specimens were taken to check the moisture content of the masonry.
Results and discussion
The test results of bulk density, water absorption and porosity of masonry materials are presented in Table 1. Two types of mortar were identified in the construction of masonry walls in the building – one type was marked as “mortar 1” and the other as “mortar 2”. In the examination of the composition of the mortars (by dissolving in hydrochloric acid), it was found that the binder-aggregate ratio for mortars used in the masonry walls of the building varied from 1:4.4 (mortar 1) to 1:2.5 (mortar 2).
Table 1.
Properties of tested bricks and mortars.
| Bulk density [g/cm3] | Water absorption (weight)(1) [%] | Water absorption (volume)(2) [%] | Skeleton density [g/cm3] | Open porosity [%] | |
|---|---|---|---|---|---|
| Bricks | 1.65 | 16.3 | 26.9 | 2.70 | 38.9 |
| Mortar 1 | 1.55 | 13.5 | 20.9 | 2.75 | 43.6 |
| Mortar 2 | 1.70 | 11.5 | 19.6 | 2.68 | 36.6 |
(1) Water absorption (weight)
.
(2) Water absorption (volume)
.
Ww – is the weight of the specimen at fully saturated condition.
Wd – is the weight of the oven-dried specimen.
Skeleton density was obtained using helium pycnometer Quantachrome Ultrapyc 1200e.
(3) Open porosity
.
The bricks and mortars collected from walls were characterised by great water absorption and porosity, which is characteristic for historic masonry materials18,28,29.
The results of strength tests on bricks and mortars are shown in Table 2.
Table 2.
The effect of water saturation of bricks and mortars on compressive strength.
| Number of specimens | Compressive strength in the air-dry condition [MPa] |
Compressive strength in the wet condition [MPa] |
kB =fB(w)/fB(a−d) [-] |
kM =fM(w)/fM(a−d) [-] |
|
|---|---|---|---|---|---|
| Bricks | 7(a-d) / 7(w) |
28.3 [0,25] |
24.4 [0,24] |
0.86 | |
| Mortar 1 | 7(a-d) / 7(w) |
6.6 [0,18] |
4.7 [0.35] |
0.71 | |
| Mortar 2 | 7(a-d) / 7(w) |
17.6 [0.09] |
13.0 [0.16] |
0.74 |
fB(w), fM(w)- mean compressive strength in the wet condition for the bricks and mortar respectively.
fB(a−d), fM(a−d)- mean compressive strength in the air-dry condition for the bricks and mortar respectively.
[…] – in square brackets the coefficients of variation of strength are given.
(a-d) – specimens in air-dry condition.
(w) – specimens in wet condition.
The compressive strength of bricks in the wet condition was 14% lower than the brick strength in the air-dry condition. Significant decreases in the compressive strength of ceramic bricks in the wet state compared to the air-dry state were obtained in the studies of T. Martins et al.14, N. Santhiparan et al.15, T. Nagarajan et al.30 and P. Matysek et al.31. The reduction in the compressive strength of bricks caused by their strong moisture content ranged from 7% to 23% (average 14.4%). These studies concerned bricks characterized by low compressive strength, which are often found in the structures of most existing buildings.
A greater reduction of strength than for bricks was obtained in tests of mortars – 29% and 26%, respectively. These results correspond well with the data of previous experiments for cement and cement-lime mortars (N. Sathiparan et al.15, A.M. Amade et al.12, J. Kubik and Z. Perkowski32,33. Full saturation of the mortar specimens resulted in a decrease of the compressive strength from 4% to 41%, i.e., significantly more than for concrete. For lime mortar, the effect of strong moisture on compressive strength was even greater and ranged from 46% to 54%14,17.
The effect of strong moisture on the compressive behavior of capillary-porous materials, such as ceramic bricks and mortars, is affected by a multitude of factors. The most important of them include the structure of the pores and the phase composition of the material.
The decrease of the material strength in the wet condition is caused by, among other things, the reduction of friction between the elements of the microstructure, weakening of inter-structural connections due to their dissolution, and the action of dewetting pressures occurring in the proximity of the phase boundary32,33,35,34.
Research on bricks taken from historical objects was conducted by J. Witzany13. Based on these experimental studies, it was found that the decrease in strength in the wet condition depends on the number of pores with small diameters in ceramic bricks; the greater the number of pores with the diameter from 0.01 μm to 1.0 μm, the greater the reduction of compressive strength. The decrease in the compressive strength of bricks in the wet condition recorded in the tests is also significantly influenced by the salinity of the ceramic material36,37. P. Foraboschi and A. Vanin36 tested bricks taken from historical structures located in Venice, confirming a 50% reduction in compressive strength of wet bricks with significant degrees of salinity in relation to bricks tested in the air-dry condition.
In the case of mortars, the strong effect of strength reduction results from the gradual dissolution and washing out of the binder, which is the basic component of the mortar. This effect is particularly strong in lime mortars exposed to long-term water contact20.
Figure 6a shows the relationship between coefficient kB and water absorption of bricks. A trend is visible: the higher the water absorption of bricks, the greater the decrease of compressive strength in the wet condition. For mortars, the relationship between coefficient kM and water absorption is less pronounced (Fig. 6b).
Fig. 6.
Reduction of compressive strength of masonry materials in the wet condition (kB, kM) vs. water absorption of materials, (a) bricks, (b) mortars.
Typical failure modes of brick and mortar specimens are presented in Fig. 7. The failure modes of the specimens in the air-dried state and the wet state did not differ significantly. although the destructive forces were definitely different.
Fig. 7.
Specimens after compression test - on the left side the specimens in the air-dry condition, on the right side the specimens in the wet condition.
Altogether, 10 brick columns were subjected to compression tests − 4 in the air-dry condition and 6 in the wet condition. In Table 3 the results of tests are shown.
Table 3.
Compressive strength of masonry.
| Column group | Mortar type | f (a−d) [MPa] | f (w) [MPa] | kMA=f (w)/f (a−d) [-] | sd [-] |
|---|---|---|---|---|---|
|
C1 C1/1(a-d); C1/2(w/B) |
Mortar 1 | 3.3 | 3.1 | 0.94 | 0.98 |
|
C2 C2/1(a-d); C2/2(w/B) |
Mortar 1 | 4.3 | 3.4 | 0.79 | 0.96 |
|
C3 C3/1(a-d); C3/2(w/B); C3/3 (w/A) |
Mortar 2 | 5.6 | 3.6 [3.4] | 0.64 [0.61] | 0.96 [0.98] |
|
C4 C4/1(a-d); C4/2(w/B); C4/3(w/A) |
Mortar 2 | 5.8 | 5.1 [5.1] | 0.88 [0.88] | 0.93 [0.93] |
C1/1(a-d); C2/1(a-d); C3/1(a-d); C4/1(a-d) – masonry columns tested in the air-dry condition C1/2(w/B); C2/2(w/B); C3/2(w/B); C4/2(w/B) – masonry columns tested in the wet condition – “method seasoning B”.
C3/3(w/A); C4/3(w/A) - masonry columns tested in the wet condition – “method seasoning A”.
f (a−d) – masonry compressive strength in the air-dry condition.
f (w) – masonry compressive strength in the wet condition.
[…] – in square brackets the values determined for columns seasoned using method A.
Table 3 also presents the results of tests for the moisture content of bricks in the columns in the wet state (sd). Brick fragments for determining the sd coefficient were taken from the columns immediately after the strength tests. As can be seen from Table 3, both methods of saturating the masonry columns with water had similar effects. The values of sd ranged from 0.93 to 0.98 (sd = 1.0 means the full water saturation state).
For all tested groups of brick columns, the strength in the wet state was lower than in the air-dry state. The decrease in compressive strength varied from 6% to 39%. For masonry columns with mortar 1, the average value of the kMA coefficient was 0.87, while for the columns with mortar 2, the average kMA value was 0.76 or 0.75, depending on the wet-seasoning method; the slightly lower value refers to seasoning method A.
The masonry walls from which the columns of groups C1 and C2 were cut used mortar with lower strength, which explains the low compressive strengths obtained in the tests.
The tested columns were collected from a brick structure erected over 120 years ago. The quality of workmanship in the masonry was poor. The joints in the masonry walls were irregular and of varying thickness (Fig. 2). The thickness of the bed joints in the masonry columns ranged from 8 mm to 32 mm, with an average of 20 mm. In some of the columns, empty spaces not filled with mortar were also visible.
The code EN 1996-1-19 provides a power formula that allows for determining the compressive strength of masonry (f) based on the strength of masonry elements (fB) and mortar (fM):
![]() |
2 |
where: K – coefficient, for brick masonry K = 0.55.
The formula (2) can be transformed into the form:
![]() |
3 |
where: f (a−d), fB(a−d), fM(a−d) - compressive strength in the air-dry condition for masonry, bricks and mortar respectively; f (w), fB(w), fM(w) - compressive strength in the wet condition for masonry, bricks and mortar respectively.
Using the notations given in Tables 2 and 3, formula (3) can be written as follows:
![]() |
4 |
where: kMA, kB, kM – coefficients of reduction of compressive strength due to strong moisture of masonry, bricks and mortar respectively.
A comparison of the experimental test results (kMA(obs)) with those calculated using formula (4) are shown in Fig. 8 and in Table 4 - differences do not exceed 15%.
Fig. 8.
Comparison of test results with calculations using formula (4).
Table 4.
Reduction of masonry compressive strength - Results of experimental tests and calculations using formulas (4) and (5).
| kB [-] |
kM [-] |
kMA(obs) [-] |
n
[-] |
kMA(4) [-] |
kMA(obs/ kMA(4) |
kMA(5) [-] |
kMA(obs)/ kMA(5) |
|
|---|---|---|---|---|---|---|---|---|
| Present | 0.86 | 0.71 | 0.87 | 2/2 | 0.81 | 1.07 | 0.81 | 1.07 |
| 0.74 | 0.76 | 2/4 | 0.82 | 0.93 | 0.82 | 0.93 | ||
| A.M. Amde et al.12 | 0.90 | 0.74 | 0.80 | 4/4 | 0.85 | 0.94 | 0.84 | 0.95 |
| 0.90 | 0.86 | 4/4 | 0.90 | 0.96 | 0.87 | 0.99 | ||
| T. Martins et al.14 | 0.82 | 0.64 | 0.85 | 5/5 | 0.76 | 1.12 | 0.77 | 1.10 |
| N. Sathiparan et al.15 | 0.85 | 0.98 | 0.76 | 6/6 | 0.89 | 0.86 | 0.87 | 0.87 |
| 0.97 | 0.83 | 6/6 | 0.88 | 0.94 | 0.87 | 0.95 | ||
| 0.84 | 0.92 | 6/6 | 0.85 | 1.09 | 0.84 | 1.10 | ||
| Mean values | 0.83 | 0.85 | 0.989 | 0.84 | 0.995 |
n – number of masonry specimens, the first number indicates the number of specimens tested in the air-dry state and the second number indicates the number of specimens tested in the wet state.
Formula (5), proposed below, is result of analyzing various power functions in order to obtain a better fit to the experimental results.
![]() |
5 |
The values of kMA coefficient calculations from Eq. (5) and obtained from the test are presented in Fig. 9 and in Table 4.
Fig. 9.
Comparison of test results with calculations using formula (5).
The results presented in Table 4 indicate that it is possible to assess the reduction of compressive strength of masonry caused by strong moisture based on the strength of bricks and mortar tested in the air-dry and wet condition with a high degree of accuracy. The differences between kMA coefficient values calculated from formula (5) and those obtained in tests amount to 13%. Only in one case does the difference exceed 10%. The differences between the experiments and the calculations based on the relationship (5) are the result of the fact that reduction in masonry strength in the wet condition is not solely the result of a reduction in brick and mortar strength. Other effects, such as the weakening of adhesion and friction forces between bricks and mortar in joints during water saturation, are also important.
Relationship (5) is presented graphically in Fig. 10.
Fig. 10.
Relationship kMA(kB, kM) according to Eq. (5)
The graphs in Fig. 10 show that the kB coefficient, which characterizes the effect of strong moisture on bricks, has the much greater impact on the level of reduction in masonry strength than the kM coefficient, which characterizes the effect of strong moisture on mortars.
The failure modes of the brick columns tested in the air-dry condition and in the wet condition are shown in Fig. 11.
Fig. 11.
Failure modes, (a) column tested in the air-dry condition, (b) column tested in the wet condition.
The forms of destruction of the masonry columns in both moisture states were similar. First, damage to the mortar at the edges of the joints was recorded. Subsequently, small vertical cracks appeared. As the load increased, vertical cracks developed over several masonry layers. In columns tested in the wet condition, the phenomenon of “water being pressed out” of the joints was observed.
The stress-strain relationships for brick columns are shown in Fig. 12. As can be seen from the graphs in Fig. 12, all relationships have a strongly non-linear characteristic with post-critical paths.
Fig. 12.
Stress-strain relationships for masonry in various moisture conditions - the stress-strain curve for each column was developed by averaging the values of records from four LVDT sensors.
The strains of the masonry columns at failure were three times greater than the strains obtained for the maximum forces. A greater deformability of masonry columns was also recorded in the wet condition, compared to those in air-dry conditions. The values of masonry modulus of elasticity in air-dry and wet conditions are presented in Table 5. Young’s modulus of the masonry was determined as a secant modulus, taking into account deformations at stresses approximately 0.1 and 0.33 times the masonry strength.
Table 5.
The effect of strong moisture on deformation characteristics of brick masonry.
| Column group | Mortar type | E (a−d) [GPa] | E (w) [GPa] | kE=E (w)/E (a−d) [-] | sd [-] |
|---|---|---|---|---|---|
|
C1 C1/1(a-d); C1/2(w/B) |
Mortar 1 | 0.89 | 0.92 | 1.03 | 0.98 |
|
C2 C2/1(a-d); C2/2(w/B) |
Mortar 1 | 1.29 | 1.46 | 1.13 | 0.96 |
|
C3 C3/1(a-d); C3/2(w/B); C3/3 (w/A) |
Mortar 2 | 1.64 | 0.73 [0.88] | 0.45 [0.54] | 0.96 [0.98] |
|
C4 C4/1(a-d); C4/2(w/B); C4/3(w/A) |
Mortar 2 | 1.31 | 0.97 [1.14] | 0.74 [0.87] | 0.93 [0.93] |
C1/1(a-d); C2/1(a-d); C3/1(a-d); C4/1(a-d) – masonry columns tested in the air-dry condition C1/2(w/B); C2/2(w/B); C3/2(w/B); C4/2(w/B) – masonry columns tested in the wet condition – “method seasoning B”.
C3/3(w/A); C4/3(w/A) - masonry columns tested in the wet condition – ‘”method seasoning A”.
E (a−d) – masonry modulus of elasticity in the air-dry condition.
E(w) – masonry modulus of elasticity in the wet condition.
[…] – in square brackets the values determined for columns seasoned using method A.
As can be seen from Table 5, for columns with mortar 1, the modulus of elasticity in the wet condition was higher than in the air-dry condition. In contrast, for columns with mortar 2, this relationship was reversed. This confirms the results of previous tests on brick masonry, which showed that strong moisture does not always lead to reduction in the modulus of elasticity - unlike compressive strength12,17,38.
Conclusions
The effect of strong moisture on compressive strength and deformability of fired-clay brick masonry was presented in the paper. Tests were performed on brick, mortar specimens and masonry columns collected from masonry of the existing building. Bricks, mortars and masonry columns were subjected to compression tests in the air-dry condition and in the wet condition. The tests on masonry materials showed the significant reduction of the compressive strength due to strong moisture. The decrease in the compressive strength of fired-clay bricks was 14%. For the tested mortars, the decreases were 26% and 29%, respectively.
Compressive strength of masonry determined in the tests of brick columns in the wet condition was lower from 6% to 39% (on average 19%) than in the tests of the masonry columns in the air-dry condition. The presented results showed that reduction of masonry strength due to strong moisture is significant and and cannot be ignored in the analysis of the bearing capacity of brick structures.
The tested masonry was characterized by a low quality of workmanship. The quality of workmanship of tested masonry differed from the requirements given in the current standards, but corresponded well with the quality of workmanship of the brick masonry inventoried in historic buildings.
In brick structures erected over the centuries, a wide variety of materials and construction techniques have been used. For this reason, individual assessments of the effect of moisture on the masonry strength should be made.
Assessment of the reduction factor based on tests of masonry columns cut out of the structure has its limitations. In brick buildings of significant historic value, it is not permissible for conservation reasons to cut out such large specimens.
The article proposes a minor-destructive method for estimating the compressive strength reduction factor of masonry in the state of strong moisture, which is based on tests of brick and mortar specimens in air-dry and wet conditions. The proposed method allows estimating the degree of reduction of brick masonry due to strong moisture with an accuracy of up to 13%.
The results of the studies discussed in the article concerned brick masonry with lime, lime-cement and cement mortars, whereas in the structures of buildings the range of materials used is much wider. Therefore, further testing and analysis is needed to confirm the validity of the proposed method for estimating the masonry strength reduction due to strong moisture.
Acknowledgements
The authors greatly acknowledge the contribution of the technical staff of the Building Materials and Structures Research Laboratory of the Cracow University of Technology.
Author contributions
P.M. Conceptualization, Methodology, Supervision, Investigations, Writing – Original Draft, Writing – Review and EditingM.W. Investigations, Prepartion of Figures.
Data availability
The datasets used and/or analyzed during the current study are available from the corresponding author upon reasonable request.
Declarations
Competing interests
The authors declare no competing interests.
Footnotes
Publisher’s note
Springer Nature remains neutral with regard to jurisdictional claims in published maps and institutional affiliations.
References
- 1.Palella, B. I., Alfano, F. R. A. & Riccio, G. Moisture in historical buildings from causes to the application of specific diagnostic methodologies. J. Cult. Herit. Volume. 61 (6/), 150–159 (2023). [Google Scholar]
- 2.Ksit, B., Szymczak-Graczyk, A. & Nazarewicz, B. Diagnostics and renovation of moisture affected historic buildings. In Civil and Environmental Engineering Reports, 1/32/2022. 59–73 (2022).
- 3.Szemiot, N., Hoła, A. & Sadowski, Ł. Assessment of the effectiveness of secondary anti-damp insulation in heritage buildings made of historic brick: The current state of knowledge, research gaps and perspectives. Herit. Sci. (2023).
- 4.Rirsch, E. & Zhang, Z. Rising damp in masonry walls and the importance of mortar properties. Constr. Build. Mater.24, pages1815–pages1820 (2010). [Google Scholar]
- 5.Hall, C. & Hoff, W. Rising damp: Capillary rise dynamics in walls. Proc. R. Soc. A 1871–1884 (2007).
- 6.Guolo, E. et al. Investigation of capillary rise in brick masonry models under controlled conditions. Constr. Build. Mater.483, 07 (2025). [Google Scholar]
- 7.Franzoni, E., Berk, B., Bassi, M. & Marrone, C. An Integrated Approach to the Monitoring of Risin Damp in Historic Brick Masonry. Vol. 370. 03 (Construction and Building Materials, 2023).
- 8.Jasieńko, J. & Matkowski, Z. Salinity and dampness of brick walls in historic buildings – Diagnostics, research methodology, rehabilitation techniques. Wiadomości Konserwatorskie 14, 43–48 (2003) (in Polish).
- 9.EN 1996-1-1:2005. Design of Masonry Structures – Part 1–1: General Rules for Reinforced and Unreinforced Masonry Structure (CEN, 2005).
- 10.EN 1052-1. Methods of Test for masonry - Part 1: Determination of Compressive Strength (CEN, 1998).
- 11.Bouška, P., Klečka, T. & Pume, D. Experimental investigation of load bearing capacity of wet masonry. In Proceedings of the XLIX Conference of KN KILIW and KN PZITB Krynica, Poland. 125–130. (2003).
- 12.Amde, A. M., Martin, J. V. & Colville, J. The effect of moisture on compressive strength and modulus of brick masonry. In Proceedings of the 13th International Brick and Block Masonry Conference, 2004, Amsterdam. (2004).
- 13.Witzany, J., Cejka, T. & Zigler, R. The effect of moisture on significant mechanical characteristics of masonry. Eng. Struct. Technol. 2, 79–85 (2010).
- 14.Martins, T., Fernández, J. & Varum, H. Influence of moisture on the mechanical properties of load-bearing adobe masonry walls. Int. J. Architect. Herit. (2018).
- 15.Sathiparan, N. & Rumeshkumar, U. Effect of moisture condition on mechanical behavior of low strength brick masonry. J. Build. Eng.17, 23–31 (2018).
- 16.Franzoni, E., Gentilini, C., Graziani, G. & Bandini, S. Compressive behaviour of brick masonry triplets in wet and dry conditions. Constr. Build. Mater.82, 05 (2015). [Google Scholar]
- 17.Bompa, D. V. & Elghazouli, A. Y. Compressive behaviour of fired-clay brick and lime mortar masonry components in dry and wet conditions. Mater. Struct. 53–60, 1–21 (2020).
- 18.Fernandes, F. M., Lourenco, P. B. & Castro, F. Ancient clay bricks: Manufacture and properties. In Materials, Technologies and Practice. Historic Heritage Structures (Bostenaru Dan, M., Přikryl, R., Török, Á. eds.) . 29–48. ( Springer, 2010).
- 19.Valek, J., Hughes, J. J. & Groot, C. J. W. P. Historic Mortars: Characterisation, Assessment and Repair. A State-of-the Art Summary, RILEM Bookseries. Vol. 7. 1–15 (Springer, 2012).
- 20.Matysek, P. Identification of Compressive Strength and Deformability of Brick Walls in Existing Buildings (Cracow University of Technology (CUT), 2014). (in Polish).
- 21.Drobiec, Ł., Grzyb, K. & Zając, J. Analysis of reasons for the structural collapse of historic buildings. Sustainability 08, 1–36 (2021).
- 22.Kroftova, K. Most frequent problems of Building structures of urban apartment buildings from 2nd half of 19th century and the start of 20th century. Buildings11, 27 (2021). [Google Scholar]
- 23.Giaquinta, M. & Giusti, E. Researches on the equilibrium of masonry structures. Arch. Ration. Mech. Anal.88, 352–392 (1985). [Google Scholar]
- 24.Iannuzzo, A., Block, P., Angelillo, M. & Gesualdo, A. A continuous energy-based numerical approach to predict fracture mechanisms in masonry structures: CDF method. Comput. Struct.257, 106645 (2021). [Google Scholar]
- 25.EN 772-1:2000. Methods of Tests for Masonry Units - Determination of Compressive Strength. (CEN, 2000).
- 26.DIN 18555-9:1999. Prüfung von Mörteln mit mineralischen Bindemitteln – Teil 9, Festmörtel: Bestimmung der Fugendruckfestigkeit, DIN (1999).
- 27.Łątka, D. & Matysek, P. Determination of mortar strength in historical brick masonry using the penetrometer test and double punch test. Materials13(12) (2020). [DOI] [PMC free article] [PubMed]
- 28.Cultrone, G. et al. Influence of mineralogy and firing temperature on the porosity of bricks. J. Eur. Ceram. Soc.24, 547–564 (2004). [Google Scholar]
- 29.Thomson, M. L., Lindqvist, J-E., Elsen, J. & Grot, C. J.W.P. Porosity of historic mortars. In Proceedings of the 13th International Brick and Block Masonry Conference, Amsterdam (2004).
- 30.Nagarajan, T., Viswanathan, S., Ravi, S., Srinivas, V. & Narayanan, P. Experimental approach to investigate the behaviour of brick masonry for different mortar ratios. In International Conference on Advances in Engineering and Technology (ICAET’2014), Singapore (2014).
- 31.Matysek, P. & Witkowski, M. Assessment of the effect of moisture on the strength of brick walls. In Materiały Budowlane 5/2013. 10–19 (2013) (in Polish).
- 32.Kubik, J. & Perkowski, Z. Accumulation of damages in porous materials. In Monograph No 178, University of Technology Opole (2005).
- 33.Perkowski, Z. Weakening of the strength of capillary-porous materials due to moisture. In Zeszyty Naukowe Politechniki Śląskiej, Seria Budownictwo z. 101, Str. 311–318 (in Polish) (2003).
- 34.Matysek, P., Stryszewska, T., Kańka, S. & Witkowski, M. The influence of water saturation on mechanical properties of ceramic bricks – tests on 19th- century and contemporary bricks. Mater. Construct. 66(323) (2016).
- 35.Neville, A. M. Properties of Concrete (Pitman Publishing, 1973).
- 36.Foraboschi, P. & Vanin, A. Experimental investigation on bricks from historical Venetian buildings subjected to moisture and salt crystallization. Eng. Fail. Anal.45, 185–203 (2014).
- 37.Stryszewska, T. & Kańka, S. Characterization of factors determining the durability of brick masonry. In Proceedings of the 17th International Brick/Block Masonry Conference (17thIB2MaC2020), 2020 Cracow, Poland (2020).
- 38.Gentilini, C., Franzoni, E., Graziani, G. & Bandini, S. Mechanical properties of fired-clay brick masonry models in moist and dry conditions. Key Eng. Mater.624, 307–312 (2015) .
Associated Data
This section collects any data citations, data availability statements, or supplementary materials included in this article.
Data Availability Statement
The datasets used and/or analyzed during the current study are available from the corresponding author upon reasonable request.