Skip to main content
Nature Communications logoLink to Nature Communications
. 2026 Feb 19;17:2928. doi: 10.1038/s41467-026-69472-3

Electrochemical initiation and chemical reaction cascades in dual-stage thermal runaway in sulfide-based all-solid-state batteries

Yuhan Wu 1,2,#, Shu Zhang 1,3,4,#, Youlong Sun 1,2,#, Lang Huang 1,2,3,4,✉, Jiahao Xu 1,2, Chengao Liu 1,2, Shanshan Zhu 1,2, Zhaoxuan Jiang 1,2, Tianyu Gong 1, Lingxiang Guo 1, Longfei Cui 1, Tao Liu 1, Jiangwei Ju 1,2,3,4, Guanglei Cui 1,2,3,4,✉
PMCID: PMC13031332  PMID: 41714639

Abstract

Sulfide all solid-state batteries represent a promising next generation energy storage technology. However, their presumed safety is challenged by the risk of thermal runaway initiating at unexpectedly low temperatures. This critical issue stems from the unstable chemical interface between the positive electrode and thiophosphate solid electrolyte, a factor often overlooked in favor of electrochemical studies. Here we demonstrate that this electrochemically formed interphase is the primary trigger for catastrophic failure, not the bulk materials. Our investigation reveals a universal two stage degradation mechanism. The first stage involves intense exothermic reactions at the interface below 160 °C, releasing heat and gases. This initiates a second stage of propagating reactions leading to thermal runaway. Crucially, we show this hazardous process can be suppressed by interface engineering. We design a stable interfacial layer using a germanium sulfur chemistry, specifically lithium germanium sulfide. This modification delivers improved thermal safety without sacrificing battery performance. Our findings have the potential to establish a forward-looking safety paradigm, shifting the focus from bulk material compatibility to interfacial stability, and provide a vital design principle for future safe solid-state batteries.

Subject terms: Energy, Batteries, Batteries


Sulfide all-solid-state batteries face thermal safety challenges. Here, authors identify the critical role of positive electrode-electrolyte interface reactions in driving thermal runaway and demonstrate that stabilizing this interface significantly enhances thermal stability.

Introduction

While modern lithium-ion batteries (LIBs) have attained high energy densities, their intrinsic safety limitations remain unresolved stemming from flammable electrolyte decomposition cascades that initiate thermal runaway (TR) chain reactions. This critical vulnerability has shifted the paradigm towards inorganic solid electrolytes (SEs), which fundamentally bypass the Arrhenius-driven pyrolysis pathways inherent to volatile organic solvents1. Recent advancements in sulfide-based solid electrolytes, particularly argyrodite Li6PS5Cl (LPSC), have positioned this material family at the forefront of all-solid-state battery (ASSB) research due to its high ionic conductivity and favorable mechanical deformability2–4. Particularly, this decade has witnessed substantial progress in LPSC-based ASSBs with synergistic developments in electrochemical stability and scalable processing developments, enabling them as leading candidates for next-generation energy storage commercialization5–7. While the significantly enhanced thermal safety is widely acknowledged as a hallmark merit of LPSC-based ASSBs, increasingly emerging evidence of paradoxical thermal failure behaviors challenges this presumed superiority. Contrary to initial expectations, LPSC-based ASSBs composed of thermally stable components exhibit exacerbated TR performance under abuse conditions, with heat propagation rates exceeding those of liquid electrolyte systems8–11. Accelerating rate calorimeter (ARC) testing of a home-made 3.8 Ah Li|LPSC|LiNi0.5Co0.2Mn0.3O2 pouch cell demonstrates an initial self-heating temperature at 163 °C, and then culminates into explosive TR at 275 °C9.This acceleration effect magnifies at pack level, where the 3 Ah ASSB configurations demonstrate TR propagation velocities 10-fold higher than commercially available LIB equivalents10. Unlike the well-characterized negative electrode-triggering TR pathways in conventional liquid-electrolyte LIBs, the safety paradox of ASSBs originates from positive electrode-electrolyte interfacial degradation dynamics, where incompatible phase boundaries initiate self-sustaining exothermic reactions at relatively low temperatures. This mechanistic inconsistency becomes particularly evident when examining delithiated oxide positive electrode|SE interfaces at abused conditions, which demonstrate divergent thermal decomposition pathways across previously reported literature. For instance, Ouyang et al. identified solid-solid interfacial reactions between delithiated NCM811 and LPSC as the primary TR trigger, where self-ignition occurs at 325 °C and the whole exothermic process is free of detectable sulfurous gas (e.g., SO2)12. Lee’s team investigated exothermic and gas-evolution behaviors in composite positive electrodes under abuse conditions, demonstrating that mechanical grinding or thermal exposure to 150°C in argon triggers TR accompanied by substantial SO2 emissions13,14. Wu et al. identified that in the LiCoO2 | LPSC system, bulk chemical reactions between delithiated positive electrode and sulfide electrolyte dominated thermal decomposition above 300°C15. Such contrasting findings spanning reaction thresholds, gaseous byproducts, and failure modes, underscore fundamental knowledge gaps in solid-state interfacial degradation mechanisms.

The thermal runaway mechanisms in sulfide-based ASSBs are governed by intertwined thermochemical and electrochemical processes at oxide positive electrode|SE interfaces. Thermochemically, bulk S-O interdiffusion directly drives interfacial reconstruction, forming metastable phosphate-sulfate phases through elemental exchange reactions16,17. Meanwhile, electrochemically-driven interfacial dynamics, particularly charge transfer and anion redox activities, critically influence thermal degradation pathways. Sulfide SEs such as LPSC, constrained by narrow electrochemical stability windows, undergo progressive oxidation during conditioning. This process generates metastable sulfur-bridged intermediates and decomposition byproducts (e.g., -S-S-, -P-S-P-, Li3PS4) that progressively destabilize interfacial integrity18,19. Fundamental band alignment analyses further reveal that the valence band maximum (VBM) of sulfide SEs lies energetically above the Fermi level of oxide positive electrodes. This interfacial energy offset drives electron transferring from positive electrode to SE and accelerates electrochemical degradation20. Under thermal abuse conditions, these electrochemically preconditioned interfaces affect thermal runaway initiation via dual pathways: (1) interfacial decomposition of sulfur species and their subsequent exothermic reactions with delithiated positive electrodes, and (2) thermally driven lattice oxygen release from delithiated oxide positive electrodes, which synergistically amplifies interfacial instability. This process further triggers self-sustaining cascades that integrate bulk-phase redox reactions, gaseous byproduct evolution (e.g., SO2, O2), and exothermic interfacial recombination, a multifaceted degradation dynamic absent in conventional liquid-electrolyte systems. Crucially, a fundamental challenge persists in quantifying the thermodynamic-kinetic interplay between bulk S-O interdiffusion and electrochemically driven interfacial decomposition, mechanistic competitors whose relative contributions remain unresolved due to the field’s disproportionate focus on bulk thermochemistry over preconditioned interface dynamics. Additionally, the sequence of gaseous emissions (SO2, O2), solid-solid reactions, and their respective heat release ratios also need to be further mapped. Establishing decoupled thermochemical/electrochemical dominance across thermal degradation stages is therefore imperative, not only to resolve mechanistic contradictions in literature but to guide interface engineering strategies that intrinsically suppress exothermic cascades.

Here, leveraging multiscale calorimetry and online gassing techniques, we systematically elucidated the specific exothermic reaction pathway induced from chemical and electrochemical reactions in NCM811 | LPSC composite, revealing a two-stage exothermic cascade. Crucially, the electrochemically conditioning evolved interphase, characterized by disulfide bridges (-S-S-), -P-S-P-, and metastable Li3PS4 phases, governs early-stage self-heating through interfacial exothermic decomposition accompanied by SO2 evolution. At high temperatures, solid-solid reactions across positive electrode|SE interface triggers sulfide oxidation and layered positive electrode disintegration, amplifying heat generation rates and leading to uncontrollable TR. This interfacial failure paradigm extends to Li10GeP2S12 (LGPS) and Li9.54Si1.74P1.44S11.7Cl0.3 (LSPSC) systems, demonstrating universal disulfide bridge induced thermal-electrochemical coupling cascade reaction. To address this, we engineer NCM811 | Li4GeS4 composite positive electrodes via Ge-S bond stabilization to elevate the thermal thresholds. Onset temperature of self-heating (Tonset) and thermal runaway temperature (Ttr) of the as-assembled ASSBs are increased from 168 °C, 228 °C to 223 °C, 312 °C compared to the counterpart of LPSC, respectively. These findings advance the fundamental understanding of thermal runaway mechanisms and establish interface thermodynamic-kinetic mapping as a critical toolkit for designing failsafe sulfide-based ASSBs.

Results and discussion

Thermal runaway characteristics of ASSBs

To mechanistically correlate the single-cell safety characteristic with material-level thermal stabilities, a thorough assessment of the thermal runaway behavior in full ASSBs is essential. Here, LPSC-based (Supplementary Fig. 1) sulfide ASSBs were assembled employing NCM811 and Li-In as electrodes, and their charge/discharge profiles showcased good electrochemical performance (Supplementary Fig. 2). The thermal safety characteristics of both fully charged (Fig. S3, 4.5 V vs. Li+/Li, 100% state of charge (SOC)) and fully discharged (2.8 V vs. Li+/Li, 0% SOC) ASSBs were analyzed using an ARC under typical heat-wait-search (HWS) conditions. Key parameters including onset temperature of self-heating (Tonset), self-heating rate (SHR), and thermal runaway temperature (Ttr, defined as the temperature point when SHR reaches 1 °C·min−1) were recorded. Apparently, violent thermal runaway was observed for the 100% SOC ASSB, with the Tonset and Ttr being 163.0 ± 8.5 °C and 231.7 ± 2.6 °C (Fig. 1a and Supplementary Fig. 4). These findings indicate that ASSBs, while demonstrating improved safety characteristics, do not entirely mitigate thermal runaway risks and remain susceptible to severe thermal propagation under abuse conditions, consistent with prior studies9. However, the fully discharged ASSB also underwent severe thermal runaway with Tonset of 239 ± 8.5 °C and Ttr of 304.7 ± 14.7 °C (Fig. 1a and Supplementary Fig. 5), further emphasizing that high thermal stability of battery materials does not necessarily equate to high safety of full cell. To pinpoint the origins of thermal instability, we systematically investigate the thermochemical compatibility and interfacial exothermic interactions between electrode materials and SE. Negative electrode material and composite positive electrode (NMC811, LPSC, and vapor-grown carbon fiber (VGCF) in a weight ratio of 70:30:3) were carefully disassembled from ASSBs in an Ar-filled glove box for ARC analysis. Initial results showed that no exothermic behavior is detected for Li-In negative electrode with LPSC up to 350 °C, indicating their good thermal stability and limited involvement of the exothermic chain reactions during elevated temperatures (Fig. 1b and Supplementary Fig. 6). However, 100% SOC composite positive electrode exhibited Tonset and Ttr of 169.3 ± 7.8 °C, and 255.3 ± 14.7 °C, which aligned with the onset self-heating of the full cell, mirroring that positive electrode/SE reactions were mainly responsible for the observed exothermic behavior of the full cell (Fig. 1b and Supplementary Fig. 7). The differing thermal runaway behaviors between isolated positive electrode materials and full cells are primarily due to electrochemical crosstalk, where reactive species like oxygen released from the positive electrode migrate to the negative electrode and trigger intense secondary reactions, combined with contrasting experimental conditions, specifically the closed system of material-level tests versus the potentially open system in cell-level tests, which significantly alters gas release and heat accumulation dynamics. Additionally, it was unexpected to find that 0% SOC composite positive electrode also generated three discontinuous exothermic processes at 228 °C, 276 °C, and 340 °C in the HWS plot (Fig. 1b and Supplementary Fig. 8), indicating complex reaction mechanisms that differed from phase transition-induced interfacial reactions observed in delithiated states. The electrode|SE reactions were further examined by ramp heating test at ARC with a heating rate of 5 °C min-1. Severe self-heating was observed in the 100% SOC composite positive electrode, with the temperature rapidly rising from 203 °C to 363 °C within just 3.9 seconds (Supplementary Fig. 9). Moreover, grinding the 100% SOC composite positive electrode in the Ar-filled glove box led to violent burning (Supplementary Fig. 10). These findings raise significant safety concerns regarding the 100% SOC composite positive electrode, as it can trigger thermal runaway under both thermal and mechanical abuse conditions. Overall, these results unveil that it is the positive electrode|SE reactions that initiate and accelerate the self-heating of the full cell, thus the following investigation will focus on decoding the specific reaction evolution path between the layered oxide positive electrode and SE.

Fig. 1. Thermal runaway characteristics of ASSBs and the corresponding pristine electrode thermal reactions.

Fig. 1

a Heat-wait-search (HWS) curves of the fully charged (100% SOC, 4.5 V vs. Li+/Li) and fully discharged (0% SOC, 2.8 V vs. Li+/Li) LiIn|LPSC | NCM811 ASSBs. b HWS curves of the electrolyte with electrodes collected from 100% SOC and 0% SOC ASSBs. c DSC and MS curves of the pristine composite positive electrode (NMC811, LPSC, and VGCF in a weight ratio of 70:30:3), inset showing typical SEM and elemental mapping images of the pristine composite positive electrode at 25 °C, 400 °C, and 500 °C. d In situ heating XRD patterns of the pristine composite positive electrode upon heating from 40 °C to 400 °C at 1 °C min-1. e XRD patterns of the pristine composite positive electrode at 25°C, 400 °C, and 500 °C. f S 2p and P 2p XPS spectra of the pristine composite positive electrode at 25°C, 400 °C, and 500 °C. g Raman spectra of the pristine composite positive electrode at 25°C, 400 °C, and 500 °C.

Material-level interfacial reactions

To unravel the complex interfacial reactions governing thermal instability in solid-state batteries, the thermochemical compatibility between pristine oxide positive electrode, SE and VGCF was firstly investigated. Utilizing a customized online accelerating rate calorimetry-mass spectrometry (ARC-MS) system and differential scanning calorimetry (DSC), we precisely tracked exothermic events and gas evolution profiles of the composite positive electrode under heating condition. Initial characterization confirmed the individual stability of NCM811 layered oxide, LPSC, and VGCF additives, with no detectable thermal decomposition below 500 °C when tested in isolation (Supplementary Fig. 11). However, when formulated into an uncycled composite positive electrode (70:30:3 mass ratio), this ostensibly stable system underwent dramatic interfacial reactions, exhibiting two distinct exothermic peaks at 373 °C and 465 °C (Fig. 1c and Supplementary Fig. 12). ARC-MS results indicated the absence of gaseous byproducts, mirroring their solid-solid reaction pathways. To further elucidate this emergent thermal sensitivity, staged heat treatments followed by microstructural analysis were conducted. Scanning electron microscopy with energy-dispersive spectroscopy (SEM-EDS) of the composite heated to 400 °C revealed nascent sulfur diffusion from LPSC into NCM811 surfaces, accompanied by oxygen migration in the reverse direction (Fig. 1c). Upon reaching 500 °C, these interdiffusion processes culminated in substantial sulfur and oxygen depletion, coinciding with the formation of nickel-sulfur and phosphorus-oxygen bonds, a transformation that aligned systematically with the hard-soft acid-base principle. Specifically, the hard acid character of phosphorus (P5+) drives preferential coordination with oxygen (O2-, hard base), while softer nickel cations (Ni3+/4+) selectively interact with sulfur anions (S2-, soft base). This chemically selective bonding behavior, rooted in Lewis acid-base interaction energetics, provides a fundamental thermodynamic rationale for the inherent incompatibility between NCM811 and LPSC components, ultimately governing their interfacial degradation dynamics under thermal abuse conditions21,22. Complementary in situ heating X-ray diffraction (XRD) analysis revealed the progressive disappearance of NCM811 (003) and (104) diffraction peaks near 373 °C, concurrent with the emergence of a (220) peak attributed to NiO formation, confirming phase transformation in non-delithiated NCM811 when thermally coupled with LPSC (Fig. 1d). Distinctive phase evolution was observed at elevated temperatures, where XRD patterns at 400 °C indicated co-formation of NiO, Li2S, and Li3PO4, attributed to the reaction between NCM811 and LPSC (Fig. 1e). Upon reaching 500 °C, complete LPSC decomposition coincided with appearance of Ni3S2 and CoS2, confirming transition metal sulfide formation through sulfur interaction with oxide components, thereby accounting for sulfur migration into NCM811. To validate the secondary exothermic mechanism involving transition metal oxide|LPSC interactions, stoichiometric NiO was mixed with LPSC mixtures and then subjected to 500 °C thermal treatment, the yielding Li2S, NiS, and Li3PO4 as reaction products convinced the critical role of rock salt transition metal oxide on contributing the second stage exothermic reactions (Supplementary Fig. 13). Concurrently, X-ray photoelectron spectroscopy (XPS), time-of-flight secondary ion mass spectrometry (TOF-SIMS) profiles detected sequential phosphate, hypophosphite, sulfate, and sulfite species generation during thermal excursions, with sulfite/sulfate signatures at 400 °C quantitatively matching sulfur diffusion trajectories (Fig. 1f, Supplementary Fig. 14). Raman spectral evolution further corroborated this interfacial degradation pathway, showing Li2S/Li2Sx and PO43- formation at 400 °C, followed by LPSC signal attenuation and SO42- emergence at 500 °C (Fig. 1g). These multimodal characterizations collectively confirm the solid-solid interfacial degradation mechanisms. Despite inherent thermal stability of individual components, the thermodynamic incompatibility between pristine NCM811 and LPSC is conclusively demonstrated to initiate exothermic interfacial reactions under thermal abuses.

Beyond bulk chemical interactions, electrochemically driven interfacial reactions are also critical factors that must be carefully considered. The inherent electrochemical instability of LPSC, manifested through its narrow stability window and valence band misalignment with NCM811, induces formation of passivating interphase comprising sulfurous species under operating potentials. Concurrently, structural destabilization of the delithiated layered oxide positive electrode tends to exacerbate interfacial reactions. To systematically evaluate these coupled phenomena, composite positive electrodes harvested from ASSBs after formation cycling, including fully charged (4.5 V vs. Li+/Li, 100% SOC) and discharged (2.8 V vs. Li+/Li, 0% SOC) states, were subjected to in situ thermal characterizations. For the 0% SOC sample, two exothermic events were recorded at 302 °C (ΔH = 81.9 ± 4.9 J·g-1,) and 379 °C (ΔH = 333.9 ± 56.2 J·g-1) (Fig. 2a and Supplementary Fig. 15). Structural evolution monitored via in situ heating XRD spectra revealed minimal crystallographic changes below 310 °C, followed by abrupt disappearance of NCM811 | LPSC diffraction peaks and concurrent NiO phase emergence at 379 °C, confirming bulk material interactions during the second exothermic phase. The absence of gaseous products throughout heating demonstrated their solid-solid reaction pathways. XPS analysis of the 310 °C-treated composite revealed diminished -P-S-P- bond intensity and complete -S-S- bond dissociation in S 2p/P 2p spectra, directly implicating electrochemical interphase decomposition as the origin of the initial exothermic event (Fig. 2b). Subsequent Ni3S2 and PO43- formation detected at 450 °C validated the reaction between NCM811 and LPSC. These findings collectively establish a bifurcated thermal degradation paradigm: the first exothermic peak arises from electrochemically formed metastable interphase breakdown, while the second originates from intrinsic NCM811 | LPSC incompatibility. The depressed decomposition threshold of interphase species (relative to bulk material reactions) underscores electrochemical preconditioning as a critical thermal risk accelerator. Complementary postmortem analyses through SEM, ex situ XRD, and Raman spectroscopy systematically corroborated these mechanistic interpretations (Supplementary Figs. 16-18). Noteworthily, the 100% SOC composite positive electrode displayed significantly enhanced interfacial reactivity under thermal stress, characterized by two sharp exothermic peaks at 209 °C and 299 °C (Fig. 2c and Supplementary Fig. 19). This process was accompanied by a markedly greater heat release (ΔH1 = 381.8 ± 16.4 J·g⁻¹, ΔH2 = 869.7 ± 89.5 J·g⁻¹) compared to the pristine and 0% SOC counterparts (Supplementary Table S1). The initial exothermic event was critically noted to align with severe self-heating behavior identified in prior ramp tests (Supplementary Fig. 9), with its early onset temperature and correlation to thermal runaway mechanisms necessitating focused investigation. In situ heating XRD analysis revealed structural evolution during these events: the first peak corresponded to phase transformation of delithiated NCM811 from layered to spinel structure, while the second marked transition to rock-salt phase alongside progressive LPSC signal attenuation. The formation of NiO occurred alongside the initial reaction of LPSC, suggesting a synergistic promotion driven by the combined effects of lattice oxygen release from the positive electrode and destabilization by sulfur species (Fig. 2c). These observations confirm delithiated positive electrode-driven initiation of thermal decomposition, with bulk solid electrolyte involvement restricted to later stages (280 °C-350 °C). Concurrent gas evolution profiles detected via ARC-MS identify SO2 (m/z = 64), CO2 (m/z = 44), CO (m/z = 28), and O2 (m/z = 32) release during the first exothermic event, implicating lattice oxygen from delithiated NCM811 in oxidative side reactions (Fig. 2c). Post-reaction characterization of samples quenched at 250 °C and 400 °C revealed mechanistic details. XPS analysis at 250 °C showed depletion of -S-S- bonds, reduced -P-S-P- intensity, and emergence of SO42-/SO22-/PO43- species, confirming electrochemical interphase participation in early exothermic processes (Fig. 2d). Conversely, 400 °C-treated samples demonstrated LPSC decomposition with NiS/CoS formation, signifying direct NCM811 | LPSC interactions. SEM-EDS mapping at 250 °C verified the reaction between NCM811 and interphase species, while 400 °C analysis revealed Ni-S and P-O bonding indicative of complete interfacial reactions (Fig. 2e). XRD phase evolution further corroborated this mechanism. (003) peak weakening/shifting below 250 °C reflected positive electrode restructuring without LPSC participation, whereas LPSC signal disappearance and NiO/NiS/Li3PO4 emergence at 400 °C confirmed bulk material interactions. Raman spectra exhibited PS43- depletion and SO42-/PO43- formation at 400 °C, consistent with the reaction between NCM811 and LPSC (Supplementary Fig. 20). Electron energy loss spectroscopy (EELS) analysis elucidated dynamic redox evolution of nickel species during thermal degradation. At 250 °C, concurrent shifts in the O K-edge pre-edge (527–534 eV) toward higher energy loss and Ni L-edge (852–858 eV) toward lower energy loss were observed, directly evidencing Ni3+/ Ni4+ reduction coupled with reactive lattice oxygen liberation. This dual electronic-state modulation mechanistically accounted for oxygen-containing gas evolution during the initial exothermic phase (Supplementary Fig. 21). Subsequent O K-edge disappearance and continued Ni L-edge shifts at 400 °C verified rock-salt phase formation. Collectively, these results establish a dual-path thermal degradation mechanism: low-temperature exothermicity arises from electrochemical interphase|lattice oxygen interactions, while high-temperature events originate from intrinsic NCM811 | LPSC incompatibility.

Fig. 2. Thermal performances of the composite positive electrodes at different SOCs.

Fig. 2

a In situ heating DSC-XRD-MS analysis of the 0% SOC composite positive electrode (NMC811, LPSC, and VGCF in a weight ratio of 70:30:3). b S 2p and P 2p XPS spectra of the 0% SOC composite positive electrode at 25 °C, 310 °C, and 450 °C. c In situ heating DSC-XRD-MS analysis of the 100% SOC composite positive electrode (NMC811, LPSC, and VGCF in a weight ratio of 70:30:3). d S 2p and P 2p XPS spectra of the 100% SOC composite positive electrode at 25°C, 250 °C, and 400 °C. e SEM and element mapping images of the 100% SOC composite positive electrode at 25 °C, 250 °C, and 400 °C. f XRD patterns of the 100% SOC composite positive electrode at 25 °C, 250 °C, and 400 °C.

To further clarify the proposed mechanisms, cross-sectional specimens of thermally treated NCM811 were prepared via focused ion beam (FIB) milling and cross-sectional polishing (CP). Comprehensive microstructural characterization was performed through SEM, electron backscatter diffraction (EBSD), and transmission electron microscopy (TEM) to map elemental distribution and phase evolution. At 250 °C, SEM-EDS analysis confirmed NCM811 particles retained Ni-O dominance without sulfur penetration into bulk regions (Fig. 3a), while EBSD mapping identified spinel-phase M3O4 (M=Ni/Co/Mn) formation within positive electrode particles (Fig. 3c). These observations collectively demonstrate that the initial exothermic event is governed by positive electrode phase transformation. Thermal escalation to 400 °C revealed substantial sulfur infiltration into NCM811 particles, evidenced by intensified S signals and attenuated O intensity in SEM-EDS (Fig. 3b). EBSD quantification detected interfacial reaction products, NiS (79.4%), Li2SO4 (18.1%), and Li3PO4 (2.5%), distributed across positive electrode cross-sections, confirming S migration from LPSC and subsequent sulfide formation (Fig. 3d). High-angle annular dark-field transmission electron microscopy (HAADF-TEM) imaging coupled with selected area electron diffraction (SAED) patterns conclusively verified spinel M3O4 at 250 °C and crystalline NiS at 400 °C (Fig. 3e, f), corroborating SEM/EBSD findings. Simulation calculations were conducted to explore the interfacial incompatibility between NCM811 and LPSC at atomic scales. According to solid-state band theory, the calculated VBM of LPSC was 1.47 eV higher than the Fermi level of NCM811, indicating that electron transfer from LPSC to NCM811 was energetically favorable (Supplementary Fig. 22). This transfer triggers the oxidative decomposition of LPSC, highlighting the inherent incompatibility between NCM811 and LPSC. Furthermore, density of states (DOS) calculations revealed significant overlap between the S 3p orbitals of LPSC and the O 2p/Ni eg orbitals of NCM811 near the Fermi level (Supplementary Fig. 23). This overlap indicates a lower energy barrier for electron exchange, further supporting the hypothesis of strong chemical incompatibility between them. Moreover, the P 2p orbitals of LPSC also showed considerable overlap with the O 2p/Ni eg orbitals of NCM811, suggesting a tendency for spontaneous chemical bonding23,24. In addition, ab initio molecular dynamics (AIMD) simulations provided critical insights into the interfacial dynamics. At 250 °C, the simulations showed that delithiated NCM811 and LPSC maintain their structural integrity, with PS43- units remaining intact (Fig. 3g and Supplementary Fig. 24). However, at 400 °C, LPSC degradation becomes evident, marked by the cleavage of PS43- bonds and the formation of P-O bonds. This convergence between multiscale computational results and experimental data strongly corroborates the proposed thermal decomposition pathways.

Fig. 3. Thermal reaction mechanisms within composite positive electrode.

Fig. 3

Cross-sectional SEM and element mapping images of the 100% SOC composite positive electrode at (a) 250 °C, and (b) 400 °C. EBSD maps of the 100% SOC composite positive electrode at (c) 250 °C, and (d) 400 °C. HAADF-STEM images and the corresponding SAED patterns of the 100% SOC composite positive electrode at (e) 250 °C, and (f) 400 °C. g AIMD simulations of the interfacial reactions between delithiated NCM811 and LPSC at 250 °C, and 400 °C. h DSC curves of different degraded components with delithiated NCM811 (De-NCM). i MS curves of different degraded components with delithiated NCM811.

At this point, the specific reaction pathway between electrochemically-derived interphase components and the delithiated positive electrode becomes critically interrogated. To decouple individual interaction mechanisms of the interphase components, strategically synthesized electrochemical degradation products were systematically investigated. Electrochemically decomposed LPSC (4.5V-(LPSC/VGCF), LPSC and VGCF in 9:1 mass ratio) was synthesized by charging an In|LPSC | (LPSC/VGCF) half-cell to 4.5 V vs. Li+/Li, with XPS and Raman spectroscopic characterization confirming the presence of -S-S- and -P-S-P- species mirroring the 100% SOC composite positive electrode’s interphase compositions (Supplementary Figs. 25 and 26). Neat delithiated NCM811 (De-NCM) collected from fully-charged liquid-electrolyte pouch cells exhibited identical structural characteristics to ASSB-derived counterparts (Supplementary Fig. 27), ensuring comparability across experimental systems. Different combinations of De-NCM mixed with other interphase components were tested under DSC and ARC-MS. Clearly, isolated De-NCM demonstrated singular exothermic initiation at 221 °C accompanied by O2 evolution (Figs. 3h-3I, Supplementary Fig. 28). The De-NCM/pristine-(LPSC/VGCF) system exhibited analogous DSC onset temperatures and oxygen release patterns, suggesting that their exothermic reactions start with phase transition of delithiated NCM while the LPSC takes part in the interaction at latter stage. Strikingly, the De-NCM/4.5V-(LPSC/VGCF) system containing electrochemical degradation products displayed accelerated thermal response, with exothermic onset at 207 °C and 263% enthalpy increase (495.8 ± 47.6 J·g-1 vs 149.2 J·g-1), concurrently evolving SO2 and O2 (Supplementary Fig. 29). Given the good thermal stability of 4.5V-(LPSC/VGCF) below 400 °C, these observations conclusively attribute early-stage heat generation and sulfurous gas evolution to reactive interphase between electrochemically-degraded LPSC and delithiated NCM811 (Supplementary Fig. 30). To probe the interfacial reaction mechanisms, individual decomposition products of LPSC, including Li₂S, S, β-Li₃PS₄ (β-LPS, Supplementary Fig. 31), and -P-S-P- species, were mixed and heated with De-NCM. DSC analysis revealed minimal influence of Li2S on primary exothermic events (no SO2 detection, Supplementary Fig. 32), although Li2S did react with delithiated NCM811 at high temperatures to produce Ni3S2 (Supplementary Fig. 33). Conversely, De-NCM/S and De-NCM/β-LPS mixtures exhibited intensified exothermicity 490.6 ± 87.1/441.4 ± 32.3 J·g-1 with predominant SO2 emission and attenuated O2 release (Fig. 3h, i, Supplementary Figs. 34 and 35). Furthermore, electrochemically decomposed LPS (4.5V-(LPS/VGCF)) was further obtained to examine the exothermic behavior of -P-S-P- species. DSC result reveals large exothermic signals of delithiated-LPS/delithiated-NCM811 (903.3 J·g-1) and P2S5/delithiated-NCM811 (2072.1 J·g-1), confirming -P-S-P- species significantly contribute to the early-stage exothermic reactions (Supplementary Fig. 36). The Fermi levels and electronic properties of the key reactive intermediates provide insight into electron transfer processes (Supplementary Table S2). Upon electrochemical oxidation (e.g., during cycling or at high voltage), LPSC decomposes into products such as elemental sulfur, Li3PS4, and polysulfides. These degradation products have distinctly different sulfur chemical environments and are more reactive with oxygen. The systematic evidence establishes electrochemical LPSC decomposition products, particularly sulfurous species, as critical initiators of early-stage exothermic cascades and exclusive SO2 sources in fully charged positive electrodes during thermal runaway propagation.

Furthermore, the influence of VGCF on thermal propagation was systematically investigated. Its relevance stems from a dual functionality within the composite positive electrode: reacting with delithiated NCM811 to generate CO and CO₂, and catalyzing the decomposition of the solid electrolyte into sulfur-containing substances. In the 100% SOC configuration, CO/CO2 evolution detected during initial exothermic events (Fig. 2c) is attributed to interfacial reactions between VGCF and delithiated NCM811. Quantitative calorimetric analysis revealed this carbon-positive electrode interaction contributes 90.8 J·g-1 (16.8% of total 541.9 J·g-1), establishing its secondary thermal role (Supplementary Fig. 37). The catalytic role of VGCF in decomposing the sulfide electrolyte was further confirmed. In cycled positive electrodes, increasing the carbon content from 0.6 wt.% to 13.0 wt.% led to a marked increase in the formation of -S-S- and -P-S-P- species as well as Li₃PS₄ (Supplementary Figs. 38–39), in agreement with previous reports of carbon-mediated SE degradation25–27. Thermal analysis of these systems with varied carbon content demonstrated a proportional escalation in exothermic enthalpy (169.2, 399.6, and 631.2 J·g⁻¹) corresponding to increased VGCF loading (0.6, 2.9, and 13.0 wt%; Supplementary Fig. 40). This correlation confirms that heat release is driven by two synergistic mechanisms: (1) direct exothermic carbon-electrode reactions producing CO/CO₂, and (2) catalytically enhanced LPSC decomposition that amplifies subsequent interfacial heat generation. This dual mechanism establishes conductive carbon as both reactant and reaction promoter in thermal runaway initiation.

Thus, the specific thermal runaway pathway in NCM811 | LPSC systems could be summarized into a staged progression: electrochemical incompatibility initiates self-heating while chemical incompatibility accelerates it. Reactive oxygen species from delithiated NCM811 preferentially react with cycling-induced interphase components (-S-S-/-P-S-P-/Li3PS4) rather than LPSC itself to start the exothermic chain reactions, producing SO2 and sulfate/phosphate species alongside CO/CO2 from VGCF oxidation. This interfacial reaction dominates initial heat generation, driving rapid exothermic escalation. Subsequent temperature rise activates the reaction between LPSC and NCM811, forming NiS, Li3PO4, and sulfate/phosphate compounds with substantial exothermic contribution. The sequential energy release, electrochemical initiation at interfaces followed by chemical amplification in bulk materials, establishes a chain reaction mechanism where electrochemical triggering and chemical acceleration synergistically drive system failure (Fig. 4a).

Fig. 4. Thermal reaction routes between NCM811 and sulfide SE.

Fig. 4

a Thermal runaway route map for 100% SOC LPSC-NCM811 composite positive electrode. b Temperature of thermal runaway between delithiated NCM811 (De-NCM) and sulfide SEs. c ΔH1 between delithiated NCM811 (De-NCM) and sulfide SEs. d Gas evolution between delithiated NCM811 (De-NCM) and sulfide SEs.

Furthermore, we also elucidated the thermal reaction mechanism of the composite positive electrode at 0% SOC to contrast with its decomposition pathway at 100% SOC. The first exothermic event at 0% SOC is attributable to the reaction between NCM and phosphorus sulfide intermediates (such as -P-S-P- bridged structures) generated from LPSC decomposition (Supplementary Figs. 41-42). Conversely, the second exothermic event is attributed to the reaction between the LPSC and NCM.

The universal applicability of the thermal degradation mechanism across different sulfide solid electrolytes was systematically evaluated (Fig. 4b-d). Specifically, we extended our investigation to Li10GeP2S12 (LGPS) and Li9.54Si1.74P1.44S11.7Cl0.3 (LSPSC) using the same methodology applied to LPSC. Composite positive electrodes were prepared in both the pristine state (De-NCM mixed with pristine SE) and the electrochemically decomposed state (De-NCM mixed with SE charged to 4.5 V). The thermal behavior of these systems was subsequently characterized using adiabatic calorimetry and gas analysis.

Both fully charged LGPS- and LSPSC-based composites exhibit significant self-heating initiating near 202 °C and 199 °C, respectively, closely matching the behavior of the LPSC system (199 °C) (Supplementary Figs. 43-46). The first exothermic peak releases 395.5 J·g-1 for the charged LGPS | VGCF composite and 419.9 J·g-1 for the LSPSC-based counterpart. Crucially, the majority of this heat (246.3 J·g-1 and 270.7 J·g-1, respectively) originates from the reaction between De-NCM and the electrochemically generated interphase species (e.g., oxidized sulfur and phosphorus compounds), rather than with the pristine electrolytes (Supplementary Fig. 47). This initial reaction stage is accompanied by significant SO2 evolution, as confirmed by mass spectrometry (Supplementary Fig. 48). In stark contrast, control samples containing De-NCM mixed with the pristine (uncharged) LGPS or LSPSC powders showed negligible exothermic activity or gas release. These results universally confirm that the primary trigger for thermal runaway is the reaction between the delithiated positive electrode and the metastable decomposition products formed at the interface during high-voltage charging, not the reaction with the bulk, pristine solid electrolyte. This validates the generalizability of our proposed degradation roadmap across different sulfide electrolytes.

Interface regulation towards safer sulfide ASSBs

The aforementioned findings, which demonstrate the critical role of interfacial interactions in initiating heat generation during early-stage thermal runaway, underscore the necessity of interfacial stabilization between NCM811 and LPSC to improve ASSB thermal safety. Positive electrode surface coating has been established as an effective mitigation strategy through the introduction of inert interfacial barriers to suppress positive electrode/SE decomposition, as documented in prior researches28,29. To evaluate this approach, ASSBs incorporating Al2O3-coated NCM811 positive electrodes (designated C-NCM, 4 nm coating thickness, Supplementary Fig. 49) were systematically investigated. Initial thermal characterization of uncycled composite positive electrodes (70:30:3 mass ratio of C-NCM, LPSC, and VGCF) revealed two elevated exothermic peaks at 408 °C and 485 °C in DSC profiles (Supplementary Fig. 50), demonstrating temperature increments compared to uncoated counterparts (373 °C and 465 °C, Fig. 1c). In situ heating XRD analysis further confirmed enhanced stability, with no phase transitions observed in coated positive electrodes below 400 °C (Supplementary Fig. 51), contrasting with prominent NiO signatures detected at 373 °C in uncoated systems (Fig. 1d). These observations indicate improved interfacial compatibility through Al2O3 modification. Post-cycling analysis of C-NCM-based ASSBs (Supplementary Fig. 52) revealed attenuated XPS signals for -S-S-, -P-S-P-, and PO43- species compared to uncoated positive electrodes at full SOC (Supplementary Fig. 53), confirming reduced electrochemical degradation. Thermal evaluation of cycled C-NCM positive electrodes through DSC, ARC-MS demonstrated partial heat release mitigation, with initial exothermic onset at 213 °C (ΔH = 318.8 J·g-1) versus 209 °C (ΔH = 399.6 J·g-1) for unmodified positive electrodes (Fig. 2c and Supplementary Fig. 54). However, persistent SO2 evolution was detected at elevated temperatures despite reduced emission quantities, accompanied by comparable self-heating profiles during ARC ramp tests (200 °C onset, Supplementary Fig. 55). These findings indicate that while surface coating partially suppresses parasitic interfacial reactions, complete thermal runaway prevention remains unachievable due to the intrinsic chemical incompatibility between layered oxide positive electrodes and sulfide SEs.

The oxidative decomposition tendency of LPSC under high-voltage conditions has been fundamentally attributed to its VBM positioning above the Fermi level of NCM811, creating inherent energy level misalignment with layered oxide positive electrodes as per solid-state band theory20. The complete resolution of this thermo-electrochemical decomposition phenomenon necessitates intrinsic material-level interfacial compatibility regulation. Phosphorus-containing sulfide SEs (LPSC, LPS, LGPS, LSPSC) universally exhibit analogous thermal safety limitations due to shared P-S bonding characteristics. According to hard-soft acid base principles, the strong affinity between hard acid phosphorus and hard base oxygen in NCM811 drives interfacial incompatibility. Compared with phosphorus, germanium (Ge) demonstrates softer acid properties with reduced thermodynamic propensity for oxygen bonding, theoretically enabling enhanced positive electrode|SE compatibility through P to Ge substitution in LGS synthesis21,30. Experimentally synthesized Li4GeS4 demonstrated room-temperature ionic conductivity of 1×10-4 S cm-1 (Supplementary Fig. 56). First-principles calculations revealed improved chemical stability between NCM811 and LGS (-0.201 eV/atom) compared with NCM811-LPSC (-0.357 eV/atom) (Fig. 5a and Supplementary Fig. 57). Energy band analysis further confirmed improved LGS/NCM811 alignment through reduced VBM-Fermi level gap versus LPSC/NCM811 (Supplementary Fig. 58). These computational predictions validate the Ge-substitution strategy for interfacial optimization. Despite these advantages, Ge-containing SEs like LGPS exhibit lithium metal incompatibility through Li-Ge alloy formation (Supplementary Fig. 59)31,32, prompting the development of LGS as ionic conductor additives rather than bulk SE replacements. XPS and DSC analysis of both De-NCM/pristine LGS and De-NCM/4.5V-(LGS-VGCF) composites revealed that LGS undergoes less electrochemical decomposition and ΔH than LPSC (Supplementary Figs. 60 and 61). The fabricated LiSi|LPSC | NCM811-LGS ASSBs demonstrated enhanced electrochemical performance with 200.8 mAh·g-1 initial discharge capacity (0.05 C, specific current:1 C = 200 mA g-1, 45 °C) and 87.4% capacity retention after 100 cycles (0.5 C, 45 °C) (Fig. 5b, Supplementary Fig. 62). Thermal safety evaluation utilized composite positive electrodes (NMC811, LGS, and VGCF in a weight ratio of 70:30:3) extracted from fully charged cells (Supplementary Fig. 63). S 2p XPS analysis revealed substantially reduced -S-S- species at LGS interfaces versus LPSC-based positive electrodes, experimentally confirming decomposition mitigation (Fig. 5c). For thermal characterizations, pristine LGS composites showed no exothermic activity below 450 °C versus LPSC’s 373 °C decomposition (Fig. 5d vs 1c, Supplementary Fig. 64). Post-cycling 0% SOC LGS composites maintained high thermal stability to 450 °C, contrasting with LPSC’s 302 °C exothermic initiation (Fig. 5d vs 2a, Supplementary Fig. 65). Charged-state LGS positive electrodes exhibited thermal runaway onset ΔH reduction (381.8 ± 16.4 to 99.9 ± 9.3 J·g⁻¹), indicating suppressed parasitic reactions (Fig. 5d vs 2c, Supplementary Fig. 19 vs 66,). These observations were further corroborated by in situ MS detection of minimal SO2 emissions from LGS systems (Fig. 5e). The ultimate validation of this interface regulation strategy emerged from full-cell thermal runaway analysis. ARC testing revealed complete elimination of severe self-heating in LGS-based systems (Supplementary Fig. 67), attributable to blocked reaction pathways between stabilized interphases and delithiated positive electrodes. Most significantly, whole-cell evaluations demonstrated substantial safety parameter improvements with Tonset/Ttr elevated to 204.0 ± 15.9/324.0 ± 9.1 °C versus baseline 163.0 ± 8.5/231.7 ± 2.6 °C (Fig. 5f, Supplementary Fig. 68). The interlinked experimental evidence collectively demonstrates that strategic manipulation of interfacial chemistry through Ge-substitution effectively decouples the chain reactions driving thermal runaway, providing critical insights for developing thermally stable ASSBs.

Fig. 5. Interfacial compatibility and thermal safety of Li4GeS4 modified composite positive electrode.

Fig. 5

a Reaction energy of NCM811-LPSC and NCM811-LGS by first-principles calculations. b Cycle performance and coulombic efficiency of LiSi|LPSC | NCM811-LGS ASSBs. c S 2p XPS spectra of the LGS composite positive electrode before and after charging to 4.5 V vs. Li+/Li (100% SOC). d DSC curves of the pristine, 0% SOC, and 100% SOC LGS composite positive electrodes. e MS curves of the 100% SOC LGS composite positive electrode. f HWS curves of the 100% SOC LiIn|LPSC | NCM811-LGS ASSBs.

This study systematically elucidates the thermal runaway mechanisms in sulfide-based all-solid-state batteries through comprehensive in situ and ex situ investigations of LPSC electrolyte|NCM811 positive electrode interactions. The experimental findings systematically demonstrate that positive electrode|electrolyte interfacial reactions govern ASSB thermal instability, with electrochemically generated interphase components (formed during cycling) reacting preferentially with delithiated NCM811 to drive initial heat generation and sulfur dioxide evolution during early-stage thermal runaway. As temperatures escalate, bulk chemical interactions between NCM811 and LPSC dramatically accelerate exothermic processes, ultimately triggering uncontrolled thermal propagation. These interfacial degradation pathways extend across other sulfide systems (LGPS, LSPSC). Moreover, by stabilizing the electrochemically formed interface through Ge-S bond engineering, the Ge-substituted LiIn|LPSC|Li4GeS4-NCM811 ASSBs demonstrate significantly enhanced safety with Tonset/Ttr increasing from 168/228 °C to 223/312 °C, validating interfacial stabilization as a critical strategy for thermally robust ASSBs. The findings provide both mechanistic insights into interface-driven failure and practical solutions for safety-enhanced solid-state batteries.

Methods

Materials preparation

Materials were procured from commercial suppliers and used without further purification. Bare and Al₂O₃-coated LiNi₀.₈Co₀.₁Mn₀.₁O₂ (>99%), lithium foil (99.99%, 50 μm), VGCF (99.9%), indium foil (99.99%, 100 μm), and silicon (99.99%) were supplied by Guangdong Canrd New Energy Technology Co., Ltd. LGPS (>99%) was obtained from Hefei Kejing Material Technology Co., Ltd., and LSPSC (>99%) from Shanghai Xianxin New Materials Technology Co., Ltd. Li₂S (99.9%) was acquired from Alfa Aesar, while LiCl (99.99%), P₂S₅ (99.9%), and GeS₂ (99.9%) were purchased from Macklin Co., Ltd. LPSC is synthesized through a mechanochemical method. A stoichiometric mixture of Li2S, P2S5, and LiCl is ball-milled (FRITSCH) at 600 rpm for 24 hours (h). The mixture was first compressed into pellets and sealed in a quartz tube. Subsequently, the pellets were annealed at 550 °C for 5 h, followed by gradual cooling to 25 °C. Finally, the annealed pellets were ground using an agate mortar to yield the Li₆PS₅Cl powder. All procedures are conducted under argon. β-L3PS4 is synthesized through a mechanochemical method. A stoichiometric mixture of Li2S and P2S5 is ball-milled at 480 rpm for 48 h, followed by heating at 300 °C for 8 h in Ar. Li4GeS4 is synthesized through a mechanochemical method. A stoichiometric mixture of Li2S and GeS2 is ball-milled at 600 rpm for 36 h, followed by heating at 500 °C for 6 h in Ar.

Electrode preparation

For the preparation of composite positive electrode powders, positive electrode materials such as LiNi0.8Co0.1Mn0.1O2 and Al2O3-coated LiNi0.8Co0.1Mn0.1O2, SEs (such as LPSC, LGPS, LSPSC, and LGS), and VGCF powders are mixed in a weight ratio of 70:30:3. The mixing process involves manual grinding for 30 minutes in a glovebox under an argon atmosphere. SE/VGCF (LPSC/VGCF, LGPS/VGCF, and LSPSC/VGCF) electrode composite powders are prepared through a mechanochemical method. A stoichiometric mixture of SE and VGCF in a weight ratio of 9:1 is ball-milled at 300 rpm for 2 h. The Li-In alloy is stored after the lithium foil (3 mm in diameter) and indium foil (8 mm in diameter) are pressed under a force of 0.5 tons for 5 minutes in a PEEK die (10 mm diameter). The Li2.5Si alloy is prepared by manually grinding the stoichiometric mixture of Si powders and lithium foil for 30 minutes in a glovebox filled with an Ar atmosphere.

Electrochemical performance

Li-In|LPSC|LiNi0.8Co0.1Mn0.1O2 ASSBs are assembled in a PEEK die (10 mm diameter). 100 mg LPSC powders are first pressed under a force of 1.6 tons as the electrolyte layer, with a thickness of 0.68 mm. Then the prepared composite positive electrode powders are added homogeneously on the top of the electrolyte layer and compressed under a force of 3.2 tons (the electrode active material loading is 17.83 mg/cm2). In the end, Li-In alloy negative electrode is added on the bottom of the LPSC layer and compressed for 2 min under a force of 0.4 tons. The stack pressure is 50 MPa during battery operation. The cycle performances are evaluated using a Neware battery test system (CT-4008Q, China) in the voltage range of 2.8 − 4.2 V (vs. Li+/Li) at 0.1 C (specific current:1 C = 200 mA g-1) and 30 °C.

Li-In|LPSC|LiNi0.8Co0.1Mn0.1O2 ASSBs are assembled for thermal runaway investigation. The ASSBs are assembled in a PEEK die (20 mm diameter). 400 mg LPSC powders are first pressed under a force of 4 tons as the electrolyte layer, with a thickness of 0.74 mm. Then the prepared composite positive electrode powders are added homogeneously on the top of the electrolyte layer and compressed under a force of 10 tons (the electrode active material loading is 36.78 mg/cm2). In the end, Li-In alloy negative electrode is added on the bottom of the LPSC layer and compressed for 2 min under a force of 1.6 tons. The stack pressure is 50 MPa during battery operation. The cycle performances are evaluated using a Neware battery test system (CT-4008Q, China) in the voltage range of 2.8 − 4.5 V (vs. Li+/Li) at 0.05 C (specific current:1 C = 200 mA g-1) and 30 °C.

SE/VGCF (LPSC/VGCF, LGPS/VGCF, and LSPSC/VGCF)/LPSC/In half-cells are assembled to obtain the SEs after electrochemical decomposition. The half-cells are assembled in a PEEK die (20 mm diameter). 400 mg LPSC powders are first pressed under a force of 4 tons as the electrolyte layer (0.74 mm in thickness). Then the prepared composite positive electrode powders are added homogeneously on the top of the electrolyte layer and compressed under a force of 10 tons (the electrode active material loading is 11.82 mg/cm2). In the end, indium negative electrode is added on the bottom of the LPSC layer and compressed for 2 min under a force of 1.6 tons. The stack pressure is 50 MPa during battery operation. The cycle performances are evaluated using a Neware battery test system (CT-4008Q, China) after charging to 4.5 V (vs. Li+/Li) at 0.05 C and 30 °C.

Li2.5Si | LPSC | LGS+LiNi0.8Co0.1Mn0.1O2 ASSB is assembled for investigating the cycling performance of the battery with LGS as an ionic conductor additive in the composite positive electrode. The ASSB is assembled in a PEEK die (10 mm diameter). 100 mg LPSC powders are first pressed under a force of 1.6 tons as the electrolyte layer (0.68 mm in thickness). Then the prepared composite positive electrode powders are added homogeneously on the top of the electrolyte layer and compressed under a force of 3.2 tons (the electrode active material loading was 9.8 mg/cm2). In the end, Li2.5Si alloy negative electrode is added on the bottom of the LPSC layer and compressed for 2 min under a force of 4 tons. The stack pressure is 50 MPa during battery operation. The cycle performances are evaluated using a Neware battery test system (CT-4008Q, China). The assembled ASSBs are activated for 2 cycles in the voltage range of 2.4 − 4.2 V at 0.05 C and 45 °C, and then undergo charge-discharge cycling in the voltage range of 2.4 − 4.2 V at 0.5 C and 45 °C.

Materials characterization

Accelerating Rate Calorimeter (ARC) and Ramp test of pouch cell and electrode-electrolyte are conducted with a BTC130 (HEL, England), equipped with a mass spectrum (MS, HPR-20, Hiden Analytical Ltd). The “Heat-Wait-Search” model starting temperature is 100 °C with a heating step of 10 °C. The self-heating rate detection limit is 0.02 °C min-1 and thermal runaway criteria is 1 °C min-1. The “Ramp” model is heated with a heating rate of 5 °C min-1 up to 400 °C. The electrode materials and SEs are carefully disassembled from ASSBs in an Ar-filled glove box. 200 mg electrode materials are transferred into the small bomb chamber made of Hastelloy alloy for Ramp test, and the released gases are analyzed by MS. All MS experiments were performed under an Ar flow at a rate of 5 mL/min. The Differential Scanning Calorimeter (DSC) measurement is conducted with a Netzsch DSC214 system from 20 °C to 500 °C with a heating rate of 5 °C min-1. Samples (~10.0 mg) with an NCM-to-SE weight ratio of 7:3, prepared under the same pressure as the composite positive electrode, were placed in a 100 μL stainless steel high-pressure sealed crucible (NETZSCH, Germany) for testing. The complementary use of ARC (with large sample mass to simulate bulk adiabatic runaway) and DSC (with small sample mass to resolve individual reactions) provides a complete picture of the thermal degradation mechanisms. Scanning electron microscopy (SEM) images of positive electrode are taken by S-4800 field emission SEM (Hitachi, Japan), operated at 10 kV and element mapping test is conducted by 7593-H (Horiba, Japan). Lab-scale X-ray diffraction (XRD) measurements are conducted using a Rigaku SmartLab X-ray diffractometer equipped with Cu Kα radiation. Temperature-resolved X-ray diffraction with an external direct heating component from room temperature up to 400 °C at a heating rate of 1 °C min-1, is tested from 10° to 70° with a scan speed of 10° min-1. Raman measurements are conducted on a Thermo Scientific spectrometer (Raman Microscope DXR) equipped with a 532 nm laser. The surface chemistry of the materials is detected by X-ray photoelectron spectroscopy (XPS, Thermo Scientific ESCA Lab 250Xi). Time-of-flight secondary ion mass spectrometry (TOF-SIMS) measurements are performed in a negative mode with a 30 keV Bi3+ primary ion beam source. Transmission electron microscope (TEM, Talos F200X) and electron energy loss epectroscopy (EELS) are taken for a detailed structural analysis. The electron backscattered diffraction (EBSD) images are acquired with Oxford C-nano. The focused ion beam (FIB) technique can cut samples and expose the cross sections of samples for TEM. The cross section polisher (CP) technique can cut samples and expose the cross sections of samples for EBSD.

Calculation method

First-principles calculations were performed using the projector-augmented wave plane-wave method, as implemented in the Vienna ab initio simulation package (VASP) via the MedeA platform33,34. The Perdew–Burke–Ernzerhof (PBE) functional under the generalized gradient approximation (GGA) was adopted for the exchange–correlation potential35. PBE + U approach is performed to calculate accurate structural properties and electronic properties with spin polarization. The effective U value was set to 6.7, 4.2, and 4.9 eV for Ni, Mn, and Co, respectively36. The plane-wave energy cutoff of 520 eV was used for structural relaxation. The conjugated gradient method is utilized to optimize the geometry with the convergence threshold of 10-5 eV in energy and 0.01 eV/Å in force, respectively. The potential decomposition reactions at the interfaces were examined along the pseudobinary phase diagrams with varying fractions of reactants37. The crystal structures of Li₆PS₅Cl, Li₂S, Li₃PS₄, P₂S₅ and Li4GeS4 were sourced from the Materials Project database. The NCM model for DFT calculations was constructed based on the LiNiO₂ structure from the Materials Project by substituting Ni atoms with Co and Mn in the appropriate stoichiometric ratio. To closely mirror the highly delithiated state of the NCM positive electrode observed in our experiments, we modeled a delithiated NCM structure with an 80% degree of delithiation. This was achieved by removing the corresponding number of lithium atoms from the pristine model. The final structure for the density of states (DOS) calculations was the lowest-energy configuration obtained after DFT relaxation.

The interfacial reaction of the positive electrode with the electrolyte at elevated temperature were simulated by ab initio molecular dynamics (AIMD). The equations of motion were integrated with the Verlet algorithm using a time step of 2 fs, and micro canonical ensemble (NVE) was used to simulate the interfacial reaction from room temperature to 500 °C. A plane-wave basis set with an energy cut-off of 520 eV and a 1 × 1 × 1 k-point mesh was used for the AIMD simulations. The AIMD simulations were performed for 2 ps. The Fermi levels of two materials obtained through VASP calculations cannot be directly compared due to the absence of a unified reference point. We employed a vacuum slab model to calculate the energy difference between the vacuum level and the Fermi level (i.e., the work function), selecting crystallographic planes with the lowest surface energy as our computational models. By aligning the vacuum levels of both materials under this vacuum slab model as a common reference benchmark and setting them as the energy zero point, we obtained and compared the numerical values of the materials’ Fermi levels relative to the vacuum level. This approach enables a meaningful comparison of the Fermi levels or VBM between the two materials.

Supplementary information

Supplementary Data 1 (24KB, zip)

Acknowledgements

This work is financially supported by the National Natural Science Foundation of China (Grant No. 52572279, received by L. H., U22A20440, received by G. C.), the Emerging Industry Cultivation Plan of Qingdao Future Industry Cultivation Project (No. 24-1-4-xxgg-7-gx, received by G. C.), the Key R&D Program of Shandong Province, China (No. 2023CXGC010302, received by G. C.), and the Taishan Scholars of Shandong Province (Nos. ts201511063, received by G. C.)

Author contributions

G. C. supervised this work. L. H. and G. C. designed this work. Y. W., Y. S. carried out the electrochemical experiments and the material characterizations. Shu. Z. performed the theoretical calculations. J. X., C. L., Shanshan. Z., Z. J., T. G., L. G., L. C., T. L. and J. J. did the data analysis. Y. W. and L. H. wrote the paper. G. C., Shu. Z., T. L. and J. J. revised the manuscript. All authors commented on the final manuscript.

Peer review

Peer review information

Nature Communications thanks Janghyuk Moon and the other, anonymous, reviewer(s) for their contribution to the peer review of this work. A peer review file is available.

Data availability

Source data are provided with this paper. Source data have been deposited in Figshare under the accession code DOI link 10.6084/m9.figshare.30461468. The computational configurations have been deposited as Supplementary Data 1.

Competing interests

The authors declare no competing interests.

Footnotes

Publisher’s note Springer Nature remains neutral with regard to jurisdictional claims in published maps and institutional affiliations.

These authors contributed equally: Yuhan Wu, Shu Zhang, Youlong Sun.

Contributor Information

Lang Huang, Email: huanglang@qibebt.ac.cn.

Guanglei Cui, Email: cuigl@qibebt.ac.cn.

Supplementary information

The online version contains supplementary material available at 10.1038/s41467-026-69472-3.

References

  • 1.Lu, P. et al. Superior all-solid-state batteries enabled by a gas-phase-synthesized sulfide electrolyte with ultrahigh moisture stability and ionic conductivity. Advanced Materials33, 2100921 (2021). [DOI] [PubMed] [Google Scholar]
  • 2.Kato, Y., Hori, S. & Kanno, R. Li10 GeP2 S12 -type superionic conductors: synthesis, structure, and ionic transportation. Advanced Energy Materials10, 2002153 (2020). [Google Scholar]
  • 3.Zhou, L., Minafra, N., Zeier, W. G. & Nazar, L. F. Innovative approaches to li-argyrodite solid electrolytes for all-solid-state lithium batteries. Acc. Chem. Res.54, 2717–2728 (2021). [DOI] [PubMed] [Google Scholar]
  • 4.Wu, J. et al. All-solid-state lithium batteries with sulfide electrolytes and oxide positive electrodes. Electrochem. Energ. Rev.4, 101–135 (2021). [Google Scholar]
  • 5.Hu, L. et al. Fusion bonding technique for solvent-free fabrication of all-solid-state battery with ultrathin sulfide electrolyte. Advanced Materials36, 2401909 (2024). [DOI] [PubMed] [Google Scholar]
  • 6.Wang Z., et al. Soft carbon-thiourea with fast bulk diffusion kinetics for solid-state lithium metal batteries. Advanced Materials, 2310395 (2023). [DOI] [PubMed]
  • 7.Ma, T. et al. High-areal-capacity and long-cycle-life all-solid-state battery enabled by freeze drying technology. Energy Environ. Sci.16, 2142–2152 (2023). [Google Scholar]
  • 8.Ge, S. et al. Quantification of lithium battery fires in internal short circuit. ACS Energy Lett. 9, 5747–5755 (2024). [Google Scholar]
  • 9.Yang, S.-J. et al. Oxygen-induced thermal runaway mechanisms of Ah-level solid-state lithium metal pouch cells. eTransportation18, 100279 (2023). [Google Scholar]
  • 10.Darmet, N., Charbonnel, J., Reytier, M., Broche, L. & Vincent, R. First experimental assessment of all-solid-state battery thermal runaway propagation in a battery pack. ACS Appl. Energy Mater.7, 4365–4375 (2024). [Google Scholar]
  • 11.Vishnugopi, B. S., Hasan, M. T., Zhou, H. & Mukherjee, P. P. Interphases and electrode crosstalk dictate the thermal stability of solid-state batteries. ACS Energy Lett. 8, 398–407 (2023). [Google Scholar]
  • 12.Rui, X. et al. Distinct thermal runaway mechanisms of sulfide-based all-solid-state batteries. Energy Environ. Sci.16, 3552–3563 (2023). [Google Scholar]
  • 13.T. Kim, et al, Critical Factors Contributing to the Thermal Runaway of Thiophosphate Solid Electrolytes for All-Solid-State Batteries. Adv Funct Materials, 2404806 (2024).
  • 14.Kim, T. et al. Thermal Runaway Behavior of Li6 PS5 Cl Solid Electrolytes for LiNi0.8 Co0.1 Mn0.1 O2 and LiFePO4 in All-Solid-State Batteries. Chem. Mater.34, 9159–9171 (2022). [Google Scholar]
  • 15.Wang, S. et al. Thermal stability between sulfide solid electrolytes and oxide positive electrode. ACS Nano16, 16158–16176 (2022). [DOI] [PubMed] [Google Scholar]
  • 16.Xiao, Y. et al. Understanding interface stability in solid-state batteries. Nat. Rev. Mater. 5, 105–126 (2019). [Google Scholar]
  • 17.Ren, F. et al. The nature and suppression strategies of interfacial reactions in all-solid-state batteries. Energy Environ. Sci.16, 2579–2590 (2023). [Google Scholar]
  • 18.Tan, D. H. S. et al. Elucidating Reversible Electrochemical Redox of Li6 PS5 Cl Solid Electrolyte. ACS Energy Lett. 4, 2418–2427 (2019). [Google Scholar]
  • 19.Schwietert, T. K. et al. Clarifying the relationship between redox activity and electrochemical stability in solid electrolytes. Nat. Mater.19, 428–435 (2020). [DOI] [PubMed] [Google Scholar]
  • 20.Banik, A. et al. Can substitutions affect the oxidative stability of lithium argyrodite solid electrolytes? ACS Appl. Energy Mater.5, 2045–2053 (2022). [Google Scholar]
  • 21.Liang, Y. et al. Challenges, interface engineering, and processing strategies toward practical sulfide-based all-solid-state lithium batteries. InfoMat4, e12292 (2022). [Google Scholar]
  • 22.Tsukasaki, H. et al. Exothermal behavior and microstructure of a LiNi1/3Mn1/3Co1/3O2 electrode layer using a Li4SnS4 solid electrolyte. Journal of Power Sources479, 228827 (2020). [Google Scholar]
  • 23.Dong, Y. & Li, J. Oxide positive electrodes: functions, instabilities, self healing, and degradation mitigations. Chem. Rev.123, 811–833 (2023). [DOI] [PubMed] [Google Scholar]
  • 24.Zhu, Y., He, X. & Mo, Y. Origin of Outstanding Stability in the Lithium Solid Electrolyte Materials: Insights from Thermodynamic Analyses Based on First-Principles Calculations. ACS Appl. Mater. Interfaces.7, 23685–23693 (2015). [DOI] [PubMed] [Google Scholar]
  • 25.Zhang, W. et al. The Detrimental Effects of Carbon Additives in Li10 GeP2 S12 -Based Solid-State Batteries. ACS Appl. Mater. Interfaces.9, 35888–35896 (2017). [DOI] [PubMed] [Google Scholar]
  • 26.Yoon, K., Kim, J.-J., Seong, W. M., Lee, M. H. & Kang, K. Investigation on the interface between Li10GeP2S12 electrolyte and carbon conductive agents in all-solid-state lithium battery. Sci. Rep. 8, 8066 (2018). [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 27.Deng, S. et al. Eliminating the Detrimental Effects of Conductive Agents in Sulfide-Based Solid-State Batteries. ACS Energy Lett. 5, 1243–1251 (2020). [Google Scholar]
  • 28.Negi, R. S. et al. Insights into the positive effect of post-annealing on the electrochemical performance of Al2 O3 -Coated Ni-Rich NCM positive electrodes for lithium-ion batteries. ACS Appl. Energy Mater.4, 3369–3380 (2021). [Google Scholar]
  • 29.Negi, R. S. et al. A Dry-Processed Al2 O3 /LiAlO2 Coating for Stabilizing the Positive electrode/Electrolyte Interface in High-Ni NCM-Based All-Solid-State Batteries. Adv Materials Inter. 9, 2101428 (2022). [Google Scholar]
  • 30.Lu, P. et al. Realizing long-cycling all-solid-state Li-In||TiS2 batteries using Li6+xMxAs1-xS5I (M=Si, Sn) sulfide solid electrolytes. Nat. Commun. 14, 4077 (2023). [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 31.Zhao, J. et al. Size-Dependent Chemomechanical Failure of Sulfide Solid Electrolyte Particles during Electrochemical Reaction with Lithium. Nano Lett. 22, 411–418 (2022). [DOI] [PubMed] [Google Scholar]
  • 32.Wenzel, S. et al. Direct Observation of the Interfacial Instability of the Fast Ionic Conductor Li10 GeP2 S12 at the Lithium Metal Negative electrode. Chem. Mater.28, 2400–2407 (2016). [Google Scholar]
  • 33.Kresse, G. & Hafner, J. Ab initio molecular-dynamics simulation of the liquid-metal-amorphous-semiconductor transition in germanium. Phys Rev B Condens Matter49, 14251–14269 (1994). [DOI] [PubMed] [Google Scholar]
  • 34.Nedjemeddine, B., Abderrahim, B. & Farida, B. Structure, microstructure and ionic conductivity of the solid solution LiTi2−xSnx(PO4)3. Physica B407, 403–407 (2012). [Google Scholar]
  • 35.John, P., Kieron, B. & Matthias, E. Generalized gradient approximation made simple. Phys. Rev. Lett.77, 3865–3868 (1996). [DOI] [PubMed] [Google Scholar]
  • 36.Ou, X., Liu, T. & Zhong, W. Enabling high energy lithium metal batteries via single-crystal Ni-rich cathode material co-doping strategy. Nat. Commun. 13, 2319 (2022). [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 37.Yi, Z., He, X. & Mo, Y. First principles study on electrochemical and chemical stability of solid electrolyte–electrode interfaces in all-solid-state Li-ion batteries. J. Mater. Chem. A.4, 3253–3266 (2016). [Google Scholar]

Associated Data

This section collects any data citations, data availability statements, or supplementary materials included in this article.

Supplementary Materials

Supplementary Data 1 (24KB, zip)

Data Availability Statement

Source data are provided with this paper. Source data have been deposited in Figshare under the accession code DOI link 10.6084/m9.figshare.30461468. The computational configurations have been deposited as Supplementary Data 1.


Articles from Nature Communications are provided here courtesy of Nature Publishing Group

RESOURCES