ABSTRACT
Infections caused by bacterial colonization and biofilm formation on wounds and dressings present critical challenges to wound care, often impeding healing. Here, we report an antibiotic‐free preventive strategy based on medical fabric coated with supramolecular antimicrobial assemblies. Using layer‐by‐layer dip coating technique, we functionalized medical fabric with polyarginine (PAR30) and hyaluronic acid (HA144) polymers, biopolymers that synergistically exhibited intrinsic antimicrobial activity. Coatings deposition and structural integrity were validated by confocal microscopy and ATR‐FTIR spectroscopy. Antibacterial performance was assessed using the AATCC100 standard test method, showed strong efficacy against both Gram‐negative and Gram‐positive clinical pathogens. In vivo wound infection models, employing bioluminescent methicillin‐resistant Staphylococcus aureus (MRSA), were used to evaluate biofilm prevention. Coated and uncoated fabrics were either pre‐inoculated with MRSA or applied to pre‐infected wounds to assess their antimicrobial and anti‐biofilm effects. The coated fabrics showed potent antibacterial activity, achieving ≥6 log‐reduction in bacterial load within 24 h compared to uncoated fabrics. Bioluminescence imaging confirmed infection development in wounds covered with uncoated fabrics, while coated fabrics prevented infection with a ≥6 log‐reduction in bacterial load on fabrics and a ≥4 log‐reduction in wound biopsies. Additionally, coated fabrics inhibited biofilm formation and bacterial proliferation in wound beds inoculated with MRSA. Comprehensive in vitro and in vivo biocompatibility assessments demonstrated the safe profile of the coated fabrics for clinical use. These findings highlight the antimicrobial efficiency of coated fabrics in minimizing bacterial colonization and biofilm formation on wounds and textiles. This safe and effective first‐in‐class, innovative approach offers a promising preventive strategy against biofilm formation and addresses antimicrobial‐resistant strains like MRSA in wound care.
Keywords: antimicrobial peptides, biocompatibility, biofilm prevention, biopolymers, coating, hemocompatibility, medical device, supramolecular assembly, wound infection
The study presents an antibiotic‐free strategy using medical fabrics coated with supramolecular assemblies of polyarginine and hyaluronic acid. These coatings showed strong antimicrobial and anti‐biofilm activity in vitro and in vivo, achieving major bacterial load reductions, including against MRSA. Biocompatibility tests confirmed safety, highlighting this approach as a promising preventive solution for wound infections and biofilm formation.

1. Introduction
Between 2018 and 2020, 12 EU Member States and one EEA country reported 19,680 surgical site infections (SSIs) from 1,255,958 surgical procedures across nine types of surgeries. The incidence of SSIs ranged from 0.6% in knee prosthesis surgeries to 9.5% in open colon surgeries, depending on the procedure type [1]. Bacterial infections are a key factor in the development of chronic SSIs, as they significantly delay wound healing by perpetuating a persistent inflammatory state and resisting therapeutic interventions [2]. Staphylococcus spp. is responsible for ∼65% of persistent infection in chronic wounds and is a major contributor to SSI complications. Chronic wound infections often involve pathogenic bacteria, including aerobic and anaerobic species, including Staphylococcus spp., Streptococcus spp. and various Proteobacteria such as Pseudomonas aeruginosa, and coliform bacteria [3].
Microorganisms may exist as free‐floating (planktonic) or as biofilm aggregates, frequently forming polymicrobial population [4]. Biofilms, responsible for nearly 80% of chronic infections according to the National Institutes of Health (NIH), consist of bacteria embedded in a self‐produced polymeric matrix. This matrix provides physical protection from the host's immune system and creates specific physiological conditions leading to a characteristic high tolerance to antibiotics [3, 5]. Biofilms are particularly concerning in chronic wounds, as a systematic review and meta‐analysis reported their prevalence to be 78.2% [6] further exacerbating wound management and recovery. A notable example of the burden of biofilm‐related infections is diabetic foot ulcers (DFUs), which affect 19% to 34% of individuals with diabetes and often leading severe complications such as infection, gangrene, amputation, and even death [7]. The immunological deficiencies in general, and particularly in diabetic patients, significantly increase their susceptibility to infection and the development of chronic, severe, and complicated infected wounds often necessitating aggressive surgical debridement [8, 9].
Debridement is a powerful tool for biofilm management due to its ability to disrupt the extracellular polymeric substance, debulking biofilm aggregates, and converting biofilm‐associated bacteria into planktonic forms, making them more susceptible to the immune system and antimicrobial therapies. It is considered as a gold standard for wound care because of its effectiveness in physically removing dead, unhealthy, and infected skin and reducing bacterial burden. However, the procedure can be painful and cause additional tissue damage. Moreover, while debridement significantly aids in biofilm disruption, it will not eliminate all bacteria or biofilm aggregates. A study analyzing bacterial loads in clean, nonhealing chronic wounds found that even wounds that appear clean after debridement may harbor bacterial counts equal to or exceeding 105 colony‐forming units (CFU) per square centimeter, a threshold often associated with infection [10].
In these scenarios, wound dressings, intended to prevent infection and aid healing, may paradoxically be contaminated with bacterial cells leading to the reformation of biofilms. These biofilms can grow unchallenged within the dressing. In these cases, medical dressings, which are essential for wound care, can inadvertently exacerbate infection risk by acting as a source of contamination and infection. The hypothesis that wound dressings may act as a reservoir promoting biofilm formation has been proposed, by Thomas et al. [11]. This concept was called the ‘ping‐pong’ effect, which described that a wound bed covered by a dressing function as a static biofilm reactor, with the underside of the dressing (abiotic surface) serving as an additional reservoir for both planktonic and biofilm‐associated bacterial cells [11, 12]. Numerous studies, employing techniques such as scanning electron microscopy (SEM), have demonstrated the presence of bacterial biofilms on wound dressings and various medical implants, including surgical sutures [13, 14, 15]. P. aeruginosa and S. aureus are prominent examples of pathogens capable of rapidly forming biofilms on wound dressings, leading to delayed wound healing and heightened infection risks [13]. This phenomenon is exacerbated by the ability of wound dressings to provide additional surface area for bacterial attachment and biofilm establishment, particularly in chronic wounds. The contamination of wound dressings often necessitates their removal, resulting in further wound debridement, increased patient discomfort.
Several modified dressings have been developed in recent years, incorporating antimicrobial agents, such as zinc nanoparticles (ZnNPs) [16], zinc oxide nanoparticles (ZnONPs) [17], and silver nanoparticles (AgNPs)[18]. While these materials show promising antibacterial properties, their use in wound care poses potential risks due to their toxicity [19, 20]. A recent study on ex vivo porcine skin has shown that silver from silver‐containing dressings can penetrate the skin, induce DNA damage, and increase the expression of stress‐related genes. The degree of effect correlated with the amount of silver present in the skin [19]. AgNPs toxicity was also evaluated using a zebrafish fin regeneration model, showing a critical adverse impact on early phases of wound healing such as epithelization and the initiation of blastema formation (for fin regeneration) [20]. Furthermore, extracts from commercialized silver‐based wound dressings significantly reduce the viability and proliferation of human skin cell lines and primary fibroblast, raising concerns about their potential cytotoxicity and impact on wound healing [21, 22, 23]. Besides, others have shown that despite the promising antibacterial effect of copper nanoparticles (CuNPs), their potential toxicity still needs to be deeply investigated [24]. Indeed, recent studies have demonstrated the low to moderate cytotoxicity of copper‐based material specifically at bactericidal doses [25]. Excess ionic copper can cause oxidative stress, inflammation, and tissue damage but when doses are controlled, the cytotoxic effect can be limited [26]. This data highlighted the importance of thorough in vivo investigation of metal toxicity and the urgent need for antimicrobial solutions that are not only effective but also non‐cytotoxic, environmentally safe, and free from antibiotics.
Antimicrobial peptides (AMPs) are naturally occurring molecules that demonstrate broad‐spectrum antimicrobial activity against microorganisms, primarily by disrupting microbial membranes, which ultimately leads to cell death [27]. With the rise of antibiotic‐resistant bacteria, AMPs present a promising alternative to traditional antibiotics. The activities of the natural AMPs can be mimicked using cationic homo‐polypeptides. Among these synthetic AMP mimic, polyarginine (PAR), a cationic homopolypeptide composed of arginine residues, has demonstrated strong antibacterial properties against both Gram‐negative and Gram‐positive bacteria [28]. Previous work [28, 29, 30, 31] have shown that poly(l‐arginine) and poly(L‐lysine), when used in combination with Hyaluronic acid (HA), can be assemble into polyelectrolyte multilayer films using the layer‐by‐layer (LbL) technique. HA, a negatively charged, biocompatible, and FDA‐approved natural polysaccharides, is known for its healing properties [32]. The self‐assembly driven process enables uniform deposition glass slide [28]. Quantitative characterization of these polyelectrolyte multilayer films has shown a strong linear relationship between the number of bilayers and resulting coating thickness. Indeed, twenty bilayers of PAR/HA coating typically reach a thickness of approximately 300 nm on glass substrates [33, 34]. This linearity enables precise control over film dimension s through tuning the number of bilayers during fabrication.
A multilayer system based on PAR with a chain length of 30 residues (PAR30) and HA exhibited strong contact‐based killing properties, significantly reducing bacterial colonization [28]. Furthermore, the interaction between PAR and HA is endothermic, distinct from other polyanionic polysaccharides, which indicates a relatively low level of electrostatic binding between the two components [28]. This endothermic, entropy‐driven association reflects a supramolecular assembly in which PAR30 chains are not rigidly immobilized within the film, but rather highly mobile. As demonstrated by Quartz Crystal Microbalance (QCM) and Fluorescence Recovery After Photobleaching (FRAP) data, the weak, dynamic binding between PAR30 and HA ensures that PAR30 chains retain significant mobility and can dynamically rearrange or diffuse toward the coating surface [28]. As results, the coating preserve a flexible, bioactive interface where PAR30 chains are continuously available to interact with bacteria upon contact [28].
Notably, HA is the only polyanion investigated for which the reaction enthalpy with PAR30 is endothermic [28]. Among, the testes systems, PAR30 exhibits the weakest interaction with HA, which contributes to the high diffusion capacity of its chains within the PAR30/HA films. This molecular characteristic underpins the efficient contact‐based killing mechanism of the coating, as the mobile PAR chains can interact more readily with bacterial membranes upon contact. Thus, the unique thermodynamic profile of the PAR/HA assembly directly supports its potent antimicrobial performance. In addition to their antimicrobial effect, PAR/HA multiplayers films have demonstrated significant anti‐inflammatory activity by suppressing the release of pro‐inflammatory cytokines from macrophages, which is crucial for mitigating excessive immune responses at wound sites [35]. This dual functionality‐combating infection while reducing inflammatory‐makes PAR/HA‐based coatings particularly valuable for medical textiles.
In this study, we aimed to develop antimicrobial coating using naturally derived, biocompatible polymers, HA and PAR, leveraging supramolecular chemistry to create functional multilayers films capable of limiting bacteria colonization and preventing biofilm formation directly on wound‐contact surfaces. Following physicochemical characterization, demonstration of homogeneity; the coated surfaces were tested against pathogenic Gram+ and Gram‐ bacteria in vitro; the supramolecular coatings have been tested in an infected wound in vivo model using antibiotic‐resistant bioluminescent bacteria, providing a clinically relevant evaluation of their efficacy under realistic infection conditions.
2. Material and methods
2.1. Fabric
Medical fabric used for wound dressings were used as test samples. This fabric exhibited two different sides: a woven side made of polypropylene (PP) and a non‐woven side composed of a blend of polypropylene and viscose.
2.2. Bacterial Strains
All strains used in this study are presented in Table S1.
2.3. Solutions. Polyelectrolytes
The polyelectrolytes used in this study included polycation—poly (L‐arginine hydrochloride) (PAR) from Alamanda Polymers, USA. PAR30 consisted of 30 arginine residues with a molecular weight (Mw) of 6.4 kDa. The polyanion employed was hyaluronic acid (HA, Mw = 144 kDa), obtained from Lifecore Biomed, USA. Buffers . Tris‐NaCl Buffer (10–150 mm) was used as rinsing buffer and to dissolve the polyelectrolytes in solution. Culture media . Both Tryptic Soy Broth (TSB) and Tryptic Soy Agar (TSA) for microbiology (VWR Chemicals) were used to grow bacteria strains. Serial dilution was either made in phosphate buffered saline (PBS) or in TSB depending on the method used. To model realistic wound dressing environment in vitro, PBS or simulated wound fluid (SWF) that consist of a ratio of 1:1 of heat‐inactivated fetal bovine serum (FBS) and peptone solution (1% peptone) was used.
2.4. Buildup of (PAR/HA)24 Films with a Dipping Robot
To construct the multilayer film, 24 bilayers of (polycation/HA) were assembled using two automated dipping robots (Riegler & Kirstein GmbH, Berlin, Germany, and Soream, Aix‐en‐Provence, France) via a layer‐by‐layer (LbL) dipping coating process. Samples measuring 2 cm × 6 cm were prepared for the LbL dip‐coating procedure. PAR30 and HA were dissolved in filtered (0.2 µm) Tris‐NaCl buffer (10 mm Tris and 150 mm NaCl; pH 7.4) at a concentration of 0.5 mg/mL for each polyelectrolyte. The fabric substrates were sequentially immersed in polycation and polyanion solutions, with an intermediate rinsing step in Tris‐NaCl buffer (10–150 mm, pH 7.4). This process was repeated to achieve a total of 24 bilayers. After assembly, the coated fabrics were air‐dried at room temperature and stored at room temperature until further use. Alternatively, in the dip‐coating process, the HA144 solution concentration was maintained at 0.5 mg/mL, while the PAR30 concentration was adjusted to 0.5, 1, 2, or 4 mg/mL for different sample sets. The automated procedure for applying 6 bilayers required approximately 15 to 20 min. To evaluate the effect of varying the number of bilayers, samples were prepared using the dip‐coating method with a fixed concentration of PAR30 (0.5 mg/mL) and HA144 (0.5 mg/mL). Samples were coated with 6, 12, 18, or 24 bilayers. The coating protocols ranged in duration from about 15 min to 1.5 h, depending on the targeted number of bilayers. After coating, all samples were air‐dried for at least 24 h prior to FTIR analysis.
2.5. FTIR
FTIR spectroscopy was conducted on the woven side made of polypropylene (PP) with an Agilent 4300 FTIR Handheld spectrometer with the diamond ATR module. Scanning was recorded on a spectral range from 4000 to 650 cm−1 with 64 background scans, 64 sample scans, a resolution of 4cm−1. Each condition was analyzed in triplicate, and multiple measurements (at least between 3 and 6) were made for each sample of each condition. The resulting spectra for each condition were averaged to produce a representative spectrum. These average spectra were then compared to identify potential differences between the conditions. All spectra underwent uniform processing, including ‘ATR correction’ in the first place, followed by the removal of C‐O (from ambient CO2) peaks using the ‘Zapping’ option, and baseline correction in addition.
2.6. Confocal Microscopy
As previously demonstrated [28], the polycation was labeled with fluorescent markers for subsequent analysis. The multilayer coating was observable by depositing 100 µL of PAR with conjugated fluorescein isothiocyanate (FITC) at a concentration of 0.5 mg/mL in NaCl‐Tris buffer onto the multilayer films for 5 min. Following the diffusion of PAR‐FITC, the films were washed and examined using a Zeiss LSM 710 confocal laser scanning microscope (Heidelberg, Germany) equipped with a x20 Plan Apochromat objective (Zeiss).
2.7. In Vitro Antimicrobial Testing (AATCC100)
The antimicrobial performance was quantified using a modified version of the AATCC Test Method 100. The materials tested for antimicrobial activity included fabric coated with antimicrobial agents and an uncoated control fabric. Uniform fabric samples measuring 2.5 cm × 2.5 cm were prepared. Each sample, whether coated or uncoated, was placed in a separate 60 mm × 15 mm petri dish. The samples were moistened and saturated with 1–2 mL of either phosphate‐buffered saline (PBS) or simulated wound fluid (SWF) to replicate a realistic wound dressing environment. The fabrics were then inoculated with bacterial cultures at a concentration of 105 CFU/mL for each microbial strain. Petri dishes were incubated at 37°C for 24 h. For immediate (0‐hour) elution tests, samples were promptly transferred to tubes containing 10 mL of PBS. Microbial cells were completely eluted from the fabrics through a series of steps: 30 s of vortexing, 30 s of sonication, and an additional 30 s of vortexing. The same elution procedure was applied to the samples incubated for 24 h. Eluted samples were serially diluted using PBS and plated on TSA plates, followed by incubation at 37°C for 18–24 h. After incubation, microbial colonies were counted, and the reduction in log CFU was calculated as described in the referenced test method.
2.8. Performance and Stability of the Coating
Accelerated aging assays were conducted on (PAR30 4 / HA144 0.5)6 and (PAR30 0.5 / HA144 0.5)24 samples. These samples were exposed to 58°C for 32 days (using the Arrhenius equation, one day at 58°C is approximately 9.85 times faster than at 25°C according to ASTM F1980) with FTIR measurements taken every 2 or 4 days. Spectra were compared to each other and to a control. At the same time, antimicrobial tests were assessed, following the AATCC100 test method by comparing with a 24 h control (i.e. uncoated non‐woven). Drying tests involved air‐dried dipped coated samples. Initial FTIR measurements were taken, followed by heating at 55°C for 5 min and repeating the FTIR measurement. This heating and measurement cycle was performed twice on each sample.
2.9. Biocompatibility
BALB/3T3 mouse fibroblast cells (ATCC CCL‐163): This cell line is widely used for cytotoxicity testing according to ISO 10993–5 and ISO 10993‐12 standards. They are suitable for evaluating wound dressings with antimicrobial properties because they are a standardized fibroblast cell line, relevant for assessing wound healing as fibroblasts play a key role in tissue repair. Cells were cultured in Dulbecco's Modified Eagle Medium (DMEM) supplemented with 10% fetal bovine serum (FBS) and 1% penicillin‐streptomycin, maintained at 37°C in a humidified atmosphere of 5% CO2. Test samples were UV‐sterilized and placed in direct contact with the confluent cell monolayer in 6‐well plates. Following a 24‐h incubation period, cell viability was evaluated using a resazurin assay (Acros Organics). Microscopic observations were performed to assess morphological changes, and the results were expressed as a percentage of cell viability relative to untreated controls.
The hemolytic activity of the peptide PAR30 was evaluated using human red blood cells (RBCs). Fresh human whole blood was centrifuged at 2500 rpm for 5 min at 4°C. The plasma was carefully removed and replaced with an equal volume of Dulbecco's Phosphate‐Buffered Saline (DPBS), and this washing step was repeated three times to eliminate residual plasma components. For the assay, 100 µL of washed RBCs were dispensed into each well of a round‐bottom 96‐well plate. An equal volume (100 µL) of test solution (either PAR30 at the desired concentration, DPBS as a negative control, or 0.1% Triton X‐100 as a positive control) was added to the corresponding wells. All conditions were tested in triplicate. The plate was incubated for 30 min at 37°C in a humidified incubator with 5% CO2. After incubation, the plate was centrifuged at 1600 rpm for 5 min to pellet intact cells. Then, 100 µL of the supernatant from each well was transferred to a new 96‐well flat‐bottom plate for absorbance measurement. Hemoglobin release, indicative of hemolysis, was quantified by measuring the optical density (OD) at 550 nm using a microplate reader (Multiskan SkyHigh, Thermo Scientific, Waltham, MA, USA). The percentage of hemolysis induced by PAR30 was calculated by comparing the absorbance of each sample to that of the positive control (Triton X‐100), which was considered to represent 100% hemolysis.
2.10. Scanning Electron Microscopy
Fabric control samples and fabric‐coated films (PAR30/HA144)24 were prepared for observation using scanning electron microscopy (SEM). Specimens were exposed to S. aureus at a concentration of 105 CFU/mL for 24 h at 37°C. (similar way to AATCC100). Following exposure, bacteria on the fabrics were fixed using a solution containing 4% paraformaldehyde (PFA) and 1% glutaraldehyde in 200 mm HEPES buffer (4‐(2‐hydroxyethyl)‐1‐piperazineethanesulfonic acid) at pH 7.4. Samples were subsequently dehydrated in a graded ethanol series with increasing concentrations: 50%, 70%, 90%, and 100%. After a critical point drying step and metallization, the samples were prepared for imaging using a Quanta 250 FEG SEM (FEI Company, Eindhoven, Netherlands).
2.11. In Vivo Model
Animals. Female SKH1 mice between the ages of 8 and 12 weeks, weighing 20–25 g were used in this study. The animals were obtained from Charles River Laboratories France. Mice were allowed to acclimatize to the environment for one week before experimentation. All the animals were kept in a well aerated room at 25 ± 2°C, fed on antibiotic‐free diet and water was provided ad libitum. Ethics statement. Animal experiments were conducted in accordance with approval of protocol number dap230046 by the committee on animal experimentation at the Institut Pasteur (CEEA89, Paris, France), in application of the European Directive 2010/63 EU. Mouse model of MRSA skin wound infection using in vivo Bioluminescence imaging. The surgical procedure was modified from previous work [36]. On day 0, the day of wounding and inoculation, mice were anesthetized with inhaled isoflurane (2%) and buprenorphine at 0.05 mg/kg was given via injection for pain management. The skin was scrubbed with iodine solution followed by an ethanol rinse. A 6.0‐mm disposable skin biopsy punch was used to create a full‐thickness skin wound overlying the thoracic spinal column and the adjacent area. Wounds were inoculated with Methicillin‐resistant Staphylococcus aureus (MRSA), Xen 31, derived from the parental strain ATCC 33591 (103 CFU; 104 CFU in 30 µL of PBS) using a micropipette. Immediately following bacterial inoculation, coated or non‐coated fabrics were applied to the contaminated wound bed. Alternatively, bacteria resuspension in TSB media (104 CFU; 105 CFU in 30 µL of PBS) were added to the fabric before application, allowing assessment of the fabric's capacity in preventing bacterial proliferation both in wound and textile. A transparent dressing (TegadermRoll; 3 M Health Care, St. Paul, MN) was placed over the wound and secured with tissue adhesive (Vetbond; 3MAnimal Care, St. Paul, MN). Bioluminescence measurements. Photon emission of the luminescent bacteria in the wound region of infected mice was quantified using a SPECTRUM‐CT imaging system (PERKIN ElmER Biosciences). After infection, mice were anesthetized by means of isofluorane inhalation, and the luminescence of the bacteria was recorded by means of a charge‐coupled device camera coupled to the LivingImage software package (version 3.1; Xenogen). A digital false‐color photon emission image was generated, and photons were counted within a constant‐defined area corresponding to the surface of the chest and encompassing the whole wound region. Photon emission was expressed as photons/s/cm2/steradian. Images shown for each experiment were directly taken from the LivingImage software, in which the color scale was identical for each individual image.
2.12. Histology Assessment of Polymer‐Treated Wounds
To assess the direct effect of polymer coatings on wound tissue, polymers were applied using a spray device. Mice received 2.5 mL of hyaluronic acid (HA, 5 mg/mL) and 2.5 mL of PAR30 (10 mg/mL) directly onto the wound surface. The effect of polymer deposition was evaluated over 48 h to assess potential toxicity. At the endpoint, skin samples were fixed in 4% paraformaldehyde (PFA) for 1 h at 4°C, embedded in OCT, cryo‐sectioned at 10 µm, and mounted onto Super‐frost slides. After PBS washes, sections were stained with hematoxylin (3 min) followed by eosin (3 min) and imaged using an Olympus VS200 slide scanner.
2.13. Skin Sampling and Cytokines Quantification
Following wound establishment and topical application of the bacterial inoculum as described above, skin biopsies were collected at 24 h post treatment (control dressing versus coated dressing). The excised skin tissues were immediately placed in sterile tubes and homogenized using a mechanical tissue grinder in ice‐cold Phosphate‐Buffered Saline (PBS) containing protease inhibitors. The homogenates were centrifuged at 10 000 × g for 10 min at 4°C, and the resulting supernatants were filtered through 0.22 µm pore‐size syringe filters to remove debris. The clarified supernatants were aliquoted and stored at –80°C until further analysis. Cytokine levels of IL‐6 and TNF‐α were quantified using commercially available ELISA kits according to the manufacturers’ protocols (Quantikine mouse IL‐6 and Quantikine mouse TNF‐α; R&D Systems, Minneapolis, MN, USA). The minimum detectable concentration was 3.1 pg/ml for IL‐6, and 3.0 pg/ml for TNF‐α.
2.14. Statistical Analysis
Data analysis was performed using Graph‐Pad Prims 9.0 (GraphPad Software, La Jolla, CA, USA). Results were expressed as means ± standard deviation (SD), and statistical analysis were conducted using unpaired Student's t‐test.
3. Results
3.1. Preparation and Characterization of PAR/HA Films
The fabric material used in this study is composed of a blend of polypropylene and viscose. Samples were either left uncoated as controls or subjected to coating using the layer‐by‐layer (LbL) dipping method with an automated dipping robot (Figure 1A), as previously described [28]. Samples were trimmed to dimensions of 5 cm × 8.5 cm to fit specific sample holders for the coating process.
FIGURE 1.

Layout and display of the LbL coating. (A) Automated robot used for the LbL dipping coating. Samples were placed on specific holders and dipped in different solution: polyarginine (0.5 mg/mL), hyaluronic acid (0.5 mg/mL) and buffer baths (Tris NaCl 10–150 mm). (B) Confocal microscopy images of (PAR/HA) coatings labeled with PAR30‐FITC (green), highlighting the coating distribution on the fabric substrate (scale bar 100 µm). This illustration is schematic and represents only the early stages of the LbL process (one layer: PAR > washing buffer > HA).
Initially, the standard LbL program was used to deposit 24‐bilayers on the fabric, requiring approximatively 13 h to complete due to the extended dipping time in buffer baths and polymers (2 min) and the controlled movement of the robotic arm. To improve efficiency, an accelerated coating program was tested, featuring fast robotic arm movement and significantly reduced dipping times in buffer baths. The optimized approach allowed for the deposit of 6‐bilayers in just 15 min, enabling a rapid yet effective coating process for comparative analysis.
The coating layers on polypropylene fibers were visualized using confocal laser scanning microscopy (CLSM) after staining with polyarginine conjugated with fluorescein isothiocyanate as a fluorophore (PAR30‐FITC). The confocal images revealed that the polypropylene fiber appeared as elongated, thread‐like structures with smooth surfaces (Figure 1B). The applied staining provided clear qualitative confirmation of the coatings' presence. The polyarginine‐FITC labeled coatings were distinctly visible as continuous fluorescent layers on the fiber surfaces, indicating successful and uniform deposition of the coating. The observed fluorescence pattern also indicated consistent coverage across the fibers, with minimal gaps or patchiness, thereby confirming the robustness of the coating application. Also, no coating material has been observed in‐between the fibers demonstrating that the coating does not interfere with the absorption capacities of the textile.
3.2. Fourier‐Transform Infrared (FTIR) Spectroscopy Analysis
To establish a reference spectral profile, multiple ATR‐FTIR measurements were performed on uncoated nonwoven polypropylene (PP) fabric. The spectra consistently showed characteristic peaks of polypropylene [37], with four distinct peaks observed between 2837 and 2950 cm− 1 corresponding to aliphatic C─H stretching vibrations (Figure 2A). These peaks are attributed to the asymmetric and symmetric stretches of C─H bonds in the methyl (CH3) and methylene (CH2) groups. Additionally, two significant peaks were detected at approximately 1375 and 1457 cm− 1, which are indicative of C─H bending vibrations, specifically the symmetric bending of CH3 and the bending of CH2 groups, respectively.
FIGURE 2.

FTIR‐ATR spectra of polypropylene (PP) and coating polymers. Each spectrum represents measurements taken from three to six different sites. (A) Spectra of fabric/polypropylene alone. (B) Spectra of polyarginine 30. (C) Spectra of hyaluronic acid (HA144, 144 kDa). (D) Overlay of all spectra, highlighting the specific peaks associated with each material.
3.3. Spectral Analysis of Coating Components
Separate spectra of HA144 and PAR30 powders were obtained and overlaid with the reference PP spectrum to predict changes following the coating application (Figure 2B,C). In comparison to the baseline PP spectrum, the coatings introduced new spectral features, particularly in the regions between 2850–3500 cm− 1, 1500–1750 cm− 1, and near 1100 cm− 1. The emergence of these peaks suggests the presence of functional groups associated with HA144 and PAR30 coatings. The PAR30 spectrum displayed marked differences relative to the PP control, particularly in the range of 3400–3050 cm− 1, where N─H stretching vibrations were prominent. Notable PAR30‐specific peaks included a strong C═O stretch at 1647 cm− 1 and an N─H bending vibration at 1541 cm− 1. In contrast, the HA144 spectrum showed distinctive O─H stretching peaks between 3300 and 3450 cm− 1 and at 1400 cm− 1, alongside N─H stretches in the 3050–3200 cm− 1 range. Additionally, overlapping peaks between HA144 and PAR30 indicated potential interactions between their functional groups, particularly in the regions associated with amide and hydroxyl groups (Figure 2D).
3.4. Effect of PAR30 Concentration on Coating Profiles
The impact of varying PAR30 concentrations on the LbL‐coated fabrics was analyzed using ATR‐FTIR (Figure S1A). Coatings prepared with PAR30 concentrations ranging from 0.5 to 4 mg/mL demonstrated distinct spectral changes compared to uncoated control samples. Specifically, new peaks emerged in the regions of 3000–3500 cm− 1 (indicative of amide/amine stretches and O─H deformations), 1500–1750 cm− 1 (associated with C═O stretches and N─H bends), and around 1100 cm− 1 (C─O stretches). As the concentration of PAR30 increased, the intensity of these peaks also rose. Notably, peaks at 3288 cm− 1 (O─H/N─H stretch), 3184 cm− 1 (N─H wag), 1652 cm− 1 (C═O stretch), and 1543 cm− 1 (N─H bend) became more pronounced, indicating a greater presence of polyarginine functional groups. This concentration‐dependent increase in peak intensity suggests that the amount of PAR30 deposited on the fabric directly correlates with the spectral features observed, reflecting a higher surface coverage of the coating.
3.5. Influence of Bilayer Numbers on Coating Profiles
The effect of increasing the number of bilayers in the LbL assembly was also evaluated using ATR‐FTIR (Figure S1B). Samples were prepared with varying bilayer counts (6, 12, 18, and 24) while maintaining a constant concentration of PAR30 (0.5 mg/mL) and HA144 (0.5 mg/mL). The results showed a clear trend where the intensity of characteristic peaks increased proportionally with the number of bilayers applied, indicating a progressive accumulation of the coating material on the substrate. Although differentiating closely related bilayer conditions, such as 6 versus 12 layers, was challenging due to overlapping spectral features, the differences became more pronounced at higher bilayer counts. At 24 bilayers, significant increases in peak intensities were observed in the regions of 3000–3500 cm− 1, 1500–1750 cm− 1, and 900–1150 cm− 1, corresponding to the amide, hydroxyl, and C─O functional groups from the coating materials. This confirmed that increasing the number of bilayers enhances the overall coating thickness and coverage, leading to more pronounced spectral signatures.
3.6. Antimicrobial Efficacy
Antimicrobial activity was assessed using ISO 20743:2021 and AATCC 100 standard methods against a range of clinically relevant bacterial strains commonly associated with wound infections, including P. aeruginosa ATCC 27853, S. aureus ATCC 25923, S. epidermidis ATCC 35984, E. coli ATCC 25922, E. faecalis ATCC 29212, and A. baumannii ATCC 19606 (Table S1). The antimicrobial efficacy of the (PAR30/HA144) coatings were evaluated by monitoring the log reduction of bacterial counts compared to uncoated control samples. The (PAR30/HA144)24 coating, applied via LbL dipping, demonstrated robust antibacterial activity, consistent with previous results on glass substrates [28] or hernia meshes [30]. Indeed, coated medical fabrics, achieved a 5 to 7 log reduction against both P. aeruginosa and S. aureus compared to untreated fabric at 24 h post‐infection (Figure 3A).
FIGURE 3.

Antimicrobial activity of raw fabric after LbL coating. Fabrics were coated with (A) 24 bilayers of (PAR30/HA144)24, or with (B) 6 bilayers of (PAR30/HA144)6. (C) Fabrics were coated with (PAR30/HA144)24 using the LbL dipping method. The antimicrobial efficacy was assessed using the ISO 20743 antimicrobial test after 24 h of exposure. The bar graph represents the log reduction in bacterial counts. The dashed line represents the limit of detection for CFU counting. Data is expressed as the mean ± standard deviation of at least 3 biological replicates and 3 technical replicates.
To streamline the process, a rapid 15‐min coating protocol using only 6 bilayers ((PAR30/HA144)6) was developed. Despite the significantly reduced coating time, this rapid approach maintained strong antimicrobial efficacy, achieving >5–6 log reductions against both P. aeruginosa and S. aureus (Figure 3B).
We tested varying concentrations of PAR30 as well as the effect of different setups for the dipping process (number of bilayers). For the concentration tests, the substrate was coated with HA144 at a constant concentration of 0.5 mg/mL, while PAR30 concentrations ranged from 0.125 to 4 mg/mL. In a separate set of experiments, we kept the PAR30 and HA144 concentrations constant and varied the number of bilayers (number of dipping) applied during the dipping process. Remarkably, all tested conditions regardless of concentration or number of layers achieved complete bacterial eradication against S. aureus and P. aeruginosa. This demonstrates that neither reducing the number of bilayers nor modifying the PAR30 concentration compromised antibacterial efficacy. These findings confirm that the coating method can be successfully optimized. This underscores the versatility and robustness of the LbL dipping technique, proving that its antimicrobial performance can be preserved even with significantly shorter application times or fewer layers.
Given that AMPs are well‐known for their broad‐spectrum activity [38], we further tested the coating efficacy against two additional Gram‐negative and two additional Gram‐positive bacteria strains (listed in Table S1) (Figure 3C). This approach allowed us to evaluate the coating performance across a diverse range of pathogens. Remarkably, the results were consistent with those observed for P. aeruginosa and S. aureus, demonstrating similar levels of bacteria eradication upon contact with the fabric.
3.7. Scanning Electron Microscopy
When observing polypropylene nonwoven fabric fibers under a SEM (Figure S2), certain areas appear melted, which is indicative of the bonding process used during manufacturing. These bonding points serve to hold the nonwoven fibers together, contributing significantly to the material's structural integrity. The bonding process involves the controlled application of heat, which melts specific regions of the polypropylene fibers. Upon cooling, these regions solidify, forming strong bonds that enhance the stability and durability of the material without compromising its flexibility. Interestingly, S. aureus biofilm clusters are easily detectable on the fabric after 24 h of contact. These clusters are predominately localized in the bonding points formed by the bonding process and within some intertwined fiber regions.
In contrast, fabrics treated with our coating (PAR30/HA144)24 showed a few individual bacteria or small microcolonies. Remarkably, these solitary bacteria exhibit a rough surface and deformations, including the presence of blebs, indicating significant stress and membrane damage. These contrast sharply with the smooth surface of bacteria observed in biofilms on untreated fabric, however consistent with previous works [39, 40]. In conclusion, the antimicrobial coating effectively prevents bacterial colonization and biofilm formation on polypropylene fabrics.
3.8. Aging Assay
To assess the coating durability an accelerated aging approach was employed. Initial FTIR measurements of a 24‐bilayer coated sample taken on day 0 showed a spectral profile consistent with previous observations, confirming the initial uniformity and composition of the coating (Figure S3). However, over time, the FTIR spectra revealed a noticeable but slight decrease of absorbance in specific regions, particularly around 3000–3500cm− 1. However, the results of the antimicrobial activity test indicate sustained antimicrobial effectiveness even after 1‐year of aging (Table 1). This confirms the coating's long‐term efficiency (1 year), supporting its reliability for extended use.
TABLE 1.
Accelerated aging assay and antimicrobial efficacy evaluation using ISO 20743 standard.
| Sample | Log10 |
|---|---|
| Control | 5.99±0.27 |
| Fabric (PAR30/HA144)24 (1 year) | < 1 a |
| Fabric (PAR30/HA144)6 (1 year) | < 1 a |
Under the limit of detection (LOD).
3.9. Biocompatibility Assessment Using BALB/3T3 Mouse Fibroblast Cells
To address technical limitation and align with the intended end‐use, a dressing prototype was developed instead of relying solely on a monolayer sample. The primary reason for this change was to ensure direct contact between the coated fabric and the cells. The cytotoxicity evaluation was conducted in compliance with ISO 10993–5 and ISO 10993‐12 standards to confirm the safety and biocompatibility of the modified fabric for potential clinical applications. Direct contact assays were performed to evaluate the biocompatibility of the antimicrobial coating on BALB/3T3 mouse fibroblast cells. To assess potential cytotoxic effects from direct contact, both control (CTR) and coated prototypes (Coated) were placed directly onto BALB/3T3 cells cultured in dishes. Cell viability and morphology were evaluated microscopically. The results showed no adverse effects on cell morphology, indicating that direct exposure to the coated fabric did not harm the cells (Figure 4B). A resazurin assay was subsequently performed to assess metabolic activity, which serves as an indirect measure of cytotoxic effects. Results were expressed as mean percentages of metabolically active cells relative to the control condition (untreated cells). The coated fabric‐maintained cell viability above the critical 70% threshold required by ISO standards (Figure 4A). Importantly, no significant cytotoxic effects were detected when compared to the 20% DMSO positive control group, further supporting the biocompatibility of the coating.
FIGURE 4.

Cell viability after 24 h of direct contact with samples. (A) Percentage of cell viability after 24 h of direct contact with samples. The dashed line indicates the 70% minimum threshold for acceptable cell viability. (B) images of cells after contact with coated and uncoated samples. Images were taken at equal distance from the contact area.
3.10. Hemolysis Assays
To evaluate the hemocompatibility of PAR30, a hemolysis assay was performed using human red blood cells (RBCs) across a concentration range of 0.98–250 µg/mL. This range was selected to encompass the minimal inhibitory concentration (MIC) of PAR30 against S. aureus, previously reported to be approximately 10–20 µg/mL [28], and to extend up to more than 10 times the MICs. PAR30 induced very low hemolytic activity across all tested concentration range. Near the MIC (15.63–31.25 µg/mL), the hemolysis remained minimal, ranging from 5.95% to 6.69%. Even at the highest tested concentration (250 µg/mL, >10x MIC), hemolysis did not exceed 17%. The positive control (0.1% Triton X‐100) caused complete hemolysis (100%), validating the assay's effectiveness, while the negative control (DPBS) resulted in minimal hemolysis, with an average of 4.71%. (Figure S4). These findings indicate that PAR30 exhibits negligible cytotoxicity toward human erythrocytes, even at concentrations well above its MIC, supporting its potential as a safe antimicrobial candidate.
3.11. In Vivo Evaluation of Antimicrobial Coated Fabric Using Mouse Wound Model
The objective of this study was to evaluate the efficacy of antimicrobial‐coated fabrics in preventing bacterial colonization and biofilm formation on both wound sites and the fabric itself. By testing these fabrics, we aimed to assess their ability to inhibit bacterial growth, maintain a clean wound environment, and thereby enhance the wound healing process. Three experimental approaches were employed (Figure 5).
FIGURE 5.

Evaluation of Coated Fabrics in Preventing and Disrupting Bacterial Contamination in Wound Models. This figure illustrates three approaches to evaluating coated fabric effectiveness in wound infection models. (1) Wounds were inoculated before fabric application to evaluate bacterial growth inhibition post‐contamination, (2) Bacterial were applied to coated or uncoated fabrics before immediate wound placement to assess colonization prevention. (3) Pre‐formed biofilms (24 h) were exposed to fabrics for another 24 h to assess biofilm disruption. Bacterial loads were then quantified.
In the first approach, bacterial suspensions of 104 to 105 CFU/mL were directly applied to the fabric, either coated or uncoated, which was then immediately placed on wounds created using a skin punch biopsy technique. This setup assessed the ability of the coating to prevent bacterial colonization and biofilm formation from the point of initial contact. The coated fabric demonstrated significant efficacy in inhibiting bacterial proliferation and biofilm formation on both the fabric itself and the wound surface (Figure 6). Notably, the coated fabric remained uncontaminated after use, showing no detectable bacterial presence (Figure 6B). Additionally, no biofilm formation was observed on wounds within the first 24 h, indicating that the antimicrobial coating effectively prevented biofilm development. These results suggest that the coated fabric can provide an effective barrier against bacterial colonization, potentially improving wound management and reducing infect ion risk.
FIGURE 6.

Bioluminescence intensity at 72 h post‐infection and bacterial load comparison. (A) The images display the bioluminescence intensity in mice wounds treated with coated (left) and non‐coated (right) fabrics, 72 h post‐infection. (B) Bioluminescence intensity at 72 h post‐infection of coated and non‐coated fabrics. The images display the bioluminescence intensity in coated (left) and non‐coated (right) fabrics, 72 h post‐infection. High luminescent intensity means significant bacterial proliferation and biofilm presence. The color scale represents radiance values (p/sec/cm2/sr). (C) Coated fabric (blue) or uncoated control (red) were contaminated with MRSA, then placed on open wound. CFU counting on wound site and fabrics itself after 72 h exposure. Error bars represent the standard deviation across replicates (n = 3 mice, 2 wounds per mouse. Statistical significance was determined using unpaired t‐test (****p < 0.005).
In the second approach, following wound creation, an inoculum of either 104 or 105 CFU/mL was applied to the wound site to create a realistic wound infection. Immediately after inoculation, either coated or non‐coated fabrics were applied to the contaminated wound. This approach enabled assessment of the coated fabric's effectiveness in inhibiting bacterial growth and biofilm development post‐contamination. The results demonstrated that wounds treated with the coated fabric had significantly lower bacterial counts compared to those covered with non‐coated fabric, underscoring the coating's ability to prevent bacterial proliferation and biofilm formation. As shown in Figure 7, bacterial loads on the coated fabric were consistently reduced across all replicates. Furthermore, bioluminescence imaging conducted 48 h post‐infection (Figure 7A,B) corroborated these findings. The coated fabric group exhibited minimal luminescent signals, indicating limited bacterial and biofilm presence, whereas the non‐coated fabric group showed high bioluminescence intensity, reflecting substantial bacterial colonization and biofilm development.
FIGURE 7.

Bioluminescence Imaging and bacterial load comparison between coated and non‐coated fabrics. (A) Bioluminescence imaging of mice wounds treated with coated (left) and non‐coated (right) fabrics. High luminescence, reflecting significant bacterial activity. In the control group, the bioluminescent signal observed outside the wound area after non‐coated fabrics removal is due to the presence of excess, highly infected exudate (drainage) (B) Ex vivo bioluminescence imaging of the dressings post‐removal. High luminescence, confirming bacterial colonization and biofilm development. The color scale represents luminescence intensity in photons/sec/cm2/sr. (C) Coated fabric (blue) or uncoated control (red) were placed over infected wounds with MRSA. CFU counting on wound site and fabric at 48 h post‐infection (PI). Error bars represent the standard deviation across replicates (n = 2 mice, 2 wounds per mouse. Data are presented as mean ± SD. Statistical significance was determined using unpaired t‐test (**** p < 0.001).
Both approaches demonstrated that the coated fabrics significantly reduced bacterial colonization and prevented biofilm formation, indicating strong antimicrobial efficacy in both preventing initial bacterial contact and controlling subsequent infection.
The effectiveness of the coated fabrics in disrupting pre‐formed biofilms was assessed by allowing a biofilm to develop on the wound bed for 24 h prior to applying either coated or uncoated fabrics. The fabrics were left in place for an additional 24 h, after which bacterial loads were quantified. As illustrated in Figure 8, the coated fabrics significantly decreased bacterial counts on both the wound surface and the fabric itself compared to uncoated controls, with a particularly pronounced reduction observed on the fabric.
FIGURE 8.

Comparison of coated fabric efficacy against pre‐formed biofilms. Coated fabric (blue) and uncoated controls (red) were applied to wounds after a 24‐h period of MRSA biofilm formation. The fabrics were then left in place for an additional 24 h. CFU counts were performed on both the wound site and the fabric after this period. Error bars represent the standard deviation across replicates (n = 3 mice, 2 wounds per mouse. Statistical significance was determined using unpaired t‐test (*** p < 0.0005).
These findings demonstrate the coated fabric's strong capacity to inhibit established biofilms. Bacterial load on the fabrics is also reduced when coating is present, which underscores the coated fabric's effectiveness in reducing contamination, thereby maintaining a cleaner wound environment and potentially promoting better wound healing outcomes.
Given the substantial reduction in bacteria burden observed with coated fabric, we next investigated whether this antimicrobial effect translated in into modulated host inflammatory response. To evaluate the impact of the antimicrobial‐coated fabric on the local inflammatory response in infected wounds (24 h Post treatment), we employed the second infection approach, in which bacterial suspensions were directly applied onto wounds which then were covered by either coated or uncoated fabric. Twenty‐four hours post‐treatment, skin tissues were harvested and homogenized for cytokine quantification. TNF‐α and IL‐6 levels in skin tissue homogenates were measured using ELISA. As expected, Figure 9 shows that wounds treated with the uncoated control fabric exhibited significantly higher TNF‐α levels compared to those treated with the antimicrobial‐coated fabric (mean ± SEM: 1443 ± 50 pg/mL vs. 490 ± 30 pg/mL; ****p < 0.0001). Similarly, IL‐6 levels were markedly elevated in the control group relative to the coated dressing group (mean ± SEM: 2001 ± 66 pg/mL vs. 581 ± 35 pg/mL; ****p < 0.0001). These findings indicate that the antimicrobial‐coated dressing effectively limited bacterial proliferation in the wound environment, thereby preventing excessive immune activation and significantly reducing the local production of pro‐inflammatory cytokines TNF‐α and IL‐6.
FIGURE 9.

Levels of pro‐inflammatory cytokines IL‐6 and TNF‐α (pg/mL). IL‐6 and TNF‐α levels were measured in wound tissue after 24 h treatment. Wounds were either non‐infected and covered with uncoated fabric (green), infected and covered with uncoated fabric (blue), or infected and covered with coated fabric (red). Error bars represent the standard deviation across replicates (n = 6 mice, 2 wounds per mouse. Statistical significance was determined using unpaired t‐test (**** p < 0.001).
To further assess whether the polymers themselves could elicit local tissue alterations, we directly exposed wounded skin to liquid polymer solutions, ensuring excess and direct contact, in absence of bacterial inoculation, and subsequently analyzed histologically. One day after lesioning, polymorphonuclear cells, including neutrophils, together with some macrophages, were evident in the wound area (Figure S5). By two days post‐lesion, both polymorphonuclear cells and macrophages had increased, and fibroblast proliferation had begun (Figure S5). Notably, no differences were observed between spray‐treated and untreated lesions, indicating that the polymer application did not alter the normal wound healing response.
4. Discussion
Traditional approaches to imparting antimicrobial activity to medical fabrics have relied on the immobilization of metallic nanoparticles, quaternary ammonium compounds, or the controlled release of antibiotics. While these methods can be effective in reducing infection, they can be associated with significant drawbacks, including immune system activation, cytotoxicity, and, particularly in the case of antibiotics, the promotion of antimicrobial resistance. In light of the challenges associated with conventional antimicrobial dressing, our primary aim was to functionalize a commonly used medical fabric to reduce bacterial colonization and early biofilm formation, key determinants to infection in wound care. Our experiments were therefore designed to establish rapid antibacterial efficacy and safety, particularly in the early stages (1–2 days), as our focus was strictly on infection prevention. This study supports supramolecular, biopolymer‐based surface coatings as a practical, antibiotic‐free alternative for medical fabrics. By targeting bacterial adhesion and early stages of biofilm development at the wound‐dressing interface, PAR30/HA144 coatings address critical failure points of standard dressing without relying on conventional biocides.
The choice of PAR30/HA144 coatings was based on prior evidence of their antibacterial efficacy and suitability for biomedical applications, as reported in in vitro [28, 29, 30] and in vivo [30] for other medical device surfaces. Our previous observations showed that PAR/HA is a biocompatible coating, that has a contact‐killing based mechanism of action [30], which strongly relies on the chain‐size dependent mobility of the polycationic PAR inside the polyanionic HA milieu [28]. Given the self‐assembly properties of the coating and the inherent adhesiveness of HA; we have previously demonstrated its successful application on other medical device relevant surfaces such as titanium [35]. One of the main advantages of such self‐assembling systems on medical textiles would be the ability to coat each fiber without having any significant effect on the pores and overall structure of the textile. Hence, herein we extend that knowledge base to medical fabric preserving mechanical properties while adding durable antimicrobial functionality. To confirm the successful deposition of the coating under industrial relevant condition, handheld FTIR spectroscopy was employed as a rapid, non‐destructive, and reliable qualitative method to detect the presence of the coating on the fabric surface. This approach was chosen because it enables straightforward verification of coating presence and uniformity, while being compatible with real‐time quality control in an industrial production setting. By leveraging layer‐by‐layer (LbL) coatings composed of polyarginine (PAR30) and hyaluronic acid (HA144), this study provides robust evidence for the efficacy, scalability, and biocompatibility of these coatings, paving the way for their clinical application in wound care.
Wound dressings are essential for management of wounds by providing a protective barrier against external contaminants and promoting the healing process. However, without antimicrobial aspects, they can also serve as a vector for infection and a niche for biofilm formation, which can lead to the release of bacteria into the wound [11]. Therefore, the development of wound dressings with antibacterial activity is essential in preventing them from becoming a potential source of infection.
In response to this concern, researchers have focused on developing wound dressings with inherent antibacterial activity. Silver‐based dressings have been widely studied for their antimicrobial properties. A study by Lansdown [41] discussed the mechanisms of action of silver in wound dressings, including its reaction with moisture in wound exudate, its release, and ability to inhibit bacterial growth and prevent biofilm formation [41]. Thomas, et al., (2003) evaluated the use of nanomaterials, such as silver nanoparticles and nanofibers, in wound dressings to impart antimicrobial properties [42].
Zinc‐bionanocomposite (nZnO‐BNC) materials showed promising antimicrobial activity through two main mechanisms 1) release of Zn2+ ions that disrupt bacterial enzyme and metabolism, 2) membrane depolarization and deformation [43]. The results demonstrated the effectiveness of these nanomaterial‐based dressings in preventing bacterial colonization and biofilm formation [43, 44]. However, those types of antimicrobial wound dressing, containing heavy metals or nanomaterials, raise concerns about biocompatibility and the environmental impact [45]. Silver, for instance, is well known for its antimicrobial properties and is commonly used in wound dressings, but its release from the dressing to the wound can lead to an altered wound healing or even renal complication and/or hepatoxicity [44]. Moreover, long term exposure to silver has been shown to have immunotoxicity particularly in a diminution in NK cells; which would have consequences for patients with chronic wounds [46, 47]. Silver in wound dressing has also been linked to allergic contact dermatitis [48].
Additionally, other materials such as iodine, polyhexamethylene biguanide (PHMB), chlorhexidine have also been investigated for their potential use in antibacterial wound dressings [49, 50, 51]. Iodine shows less cytotoxicity than silver, but its systemic absorption can be a risk to provoke thyroid damage, especially for immunocompromised patients [49]. For PHMB, it was shown that it can stimulate the emergence of adaptative cross‐resistance to gentamicin in E. coli biofilms [50]. Similarly, exposure to sub‐inhibitory concentrations of chlorhexidine induced the expression of the MexXY efflux pump in P. aeruginosa, leading to the development of cross‐resistance to antibiotics such as polymyxins, cephalosporins, and fluroquinolones [51].
An alternative to those potential issues is the use of the antimicrobial properties from natural polymers such as antimicrobial peptides. AMPs are less prone to inducing resistance or cross resistance compared to traditional antibiotics [52]. Super‐resolution microscopy revealed that PAR30 chains accumulate on the bacterial membrane, destabilizing it and causing rapid lysis without entering the cells [30]. This confirms a direct contact‐killing antibacterial mechanism. The rapid, broad‐spectrum mode of action, combined with non‐specific targets, make it challenging for bacteria to adapt and develop resistance [53]. Indeed, PAR30 does not induce resistance in S. aureus, the MICs values were stable over 30 days whereas tetracycline MICs values increased by around 3 times over the same period [30].
Additionally, when combined with hyaluronic acid (HA), PAR/HA films showed strong inhibitory effects on the release of pro‐inflammatory cytokines by primary human macrophages, and keeping them in M0 naive state. This suggests their potential to reduce chronic inflammatory reaction associated with medical device implantation without compromising the clearance of bacteria by the innate immune system. Beyond exhibiting strong antimicrobial activity in vitro, PAR/HA films have been shown to be a suitable substrate for endothelial, epithelial, and connective tissue cells [30, 35]. Furthermore, PAR not only promoted cells adhesion, epithelization and angiogenesis but also demonstrated a strong potential in eliminating implanted medical device infections in vivo using an infected polymeric mesh hernia repair model [30].
In this study, our findings underscore the effectiveness of PAR30/HA144 films build on medical fabrics in preventing bacterial colonization and biofilm formation. HA forms a hydrated matrix, acting as a protective barrier, trapping bacteria, preventing their attachment to wound beds, thereby limiting bacterial growth [54]. The hydrated nature of HA also provides a biofouling effect [55], while it has been previously shown that the degradation of HA by bacteria can be used to trigger innate immune response for microbial clearance [54]. On the other hand, antimicrobial peptide directly interacts with the microorganisms, destabilize their cell membrane, and inducing bacteria death [30, 56]. In the preset study, film durability was further assessed through an aging assay, providing additional insight into the long‐term performance. This offering a more robust verification of shelf‐life, which is critical for industrial implementation and regulatory compliance.
For this work, we primarily focused on the prevention of bacterial colonization, a critical early step in biofilm formation and a well‐established target in antibiofilm strategies [57]. We also directly addressed antibiofilm efficacy in biologically relevant scenarios. Test were designed to mimic clinically relevant infection risks. First, we simulated a realistic wound environment where residual bacteria may remain even after clinical cleaning. Our coated fabrics were effective in preventing the proliferation and biofilm formation of these remaining bacteria. Second, we assessed whether the dressing itself could serve as a vector for infection. We observed that placing bacteria directly onto uncoated medical fabrics could lead to bacterial proliferation within the wound site. In contrast, the coated fabrics prevented this contamination pathway. Finally, in Approach 3, we evaluated the ability of the coated fabric to prevent and disrupt pre‐biofilms in a more complex in vivo model. Although it is uncommon for an infected wound to be dressed without prior cleaning, we deliberately used this as a worst‐case scenario. Biofilms were allowed to develop on wound beds for 24 h before treatment, mimicking a pre‐established severe infection. The application of coated fabrics led to a significant reduction in bacterial burden, as confirmed by both bioluminescence imaging and CFU counts. These results provide strong evidence of the coating's antibiofilm efficacy in both preventing initial colonization and reducing mature biofilms in a clinically relevant setting.
This also highlights the dual functionality of the coatings: preventing bacterial adhesion on fabric and bacteria proliferation on wounds. These capabilities are particularly significant given the fact that bacterial load can persist in wounds even after cleaning [10]. The increasing prevalence of biofilm in chronic wounds complicates wounds healing and often resists conventional therapies [6]. Recent studies have shown that 40% of chronic wound specimens contained biofilm aggregates with predominance of S. aureus [4]. Bioluminescence imaging provided a dynamic and quantitative assessment, confirming that the coatings not only reduce bacterial load on the fabric but also mitigate the risk of biofilm recurrence. These outcomes align with the hypothesis that antimicrobial surface coatings can break the “ping‐pong” cycle of bacterial transfer between dressings and wounds, offering a practical solution to a longstanding problem in wound management.
The ionic charges of the polymers facilitate a strong interaction with textile fibers allowing efficient and a long‐term stability of the coatings, demonstrated by the accelerated aging assays, further reinforces their practical viability. Importantly, biocompatibility testing confirmed that the coatings are safe for fibroblast cells, meeting ISO standards and supporting their suitability for clinical use. Additionally, hemolysis assays demonstrated minimal red blood cell lysis at concentrations exceeding 10 times the MIC, further confirming the hemocompatibility of PAR30‐based coatings. In comparison, AgNPs, have been shown to induce hemolysis and significantly impaired the proliferation and viability of lymphocytes [58, 59]. PAR30, however, exhibit a markedly safer profile, underscoring its promise for integration into biomedical applications. Importantly, the observed antimicrobial activity was accompanied by a significant attenuation of the local inflammatory response in vivo. While a decrease in inflammation is expected as bacterial burden is reduced, the markedly lower levels of pro‐inflammatory cytokines TNF‐α and IL‐6 in wounds treated with the coated dressing indicate that the coating achieves infection control without triggering unnecessary immune activation. This dual effect, limiting both microbial proliferation and inflammatory signaling, highlights the therapeutic potential of PAR30‐based coatings for safe and effective management of infected wounds. Building in this strong biocompatibility and safety profile, the coating process itself also emphasizes sustainability and simplicity. The application requires only aqueous solutions of fully biodegradable biopolymers, significantly reduction potential health or environmental risks and aligning with the Safe and Sustainable by Design Framework. Furthermore, by effectively preventing bacterial colonization and biofilm formation, these non‐antibiotic coating not only help reduce infections risks but also support global efforts to combat antimicrobial resistance.
To our knowledge, this is the first demonstration that PAR30/HA144 supramolecular coatings can be applied to medical fabrics substrate. Their strong antimicrobial activity against clinically relevant pathogens, including MRSA, highlight their potential to combat ESKAPE pathogens, one of the most critical groups contributions to hospital‐acquired infection and antibiotic resistance. In addition, the biocompatibility of coated fabric, offer a safe, free‐antibiotic solution for infections prevention in wound care. Future research should focus on expanding their applications, optimizing their integration into diverse clinical settings, and exploring their potential to mitigate antibiotic resistance. Collectively, these findings pave the way for the development of next generation wound dressings that enhance patient outcomes and set new standards in wound care.
Conflicts of Interest
Yes. A Diarrassouba, C Calligaro, L Petit C Guilbaud‐Chéreau, P Lavalle, Nihal Engin Vrana, and Skander Hathroubi employment SPARTHA Medical, A Vigué, employment Paul Hartmann SAS and M Kettel, Michael Karl employment Paul Hartmann AG.
Supporting information
Supporting File: adhm70783‐sup‐0001‐SuppMat.docx.
Acknowledgements
The authors would like to express their gratitude to the team at SPARTHA Medical for their valuable contributions to this work. Special thanks to Xavier Wurtz for his contributions to the illustrations. Authors would like to thank Vincent Ball (INSERM UNIT 1121) for his precious help for the FTIR experiments and Eric Mathieu (INSERM UNIT 1121) for the SEM images. Authors would also like to thank Yijie Li for the technical assistance on the coating process. This work was supported by the European Innovation Council (EIC) under the SPARTHACUS project (190184905) This project has received funding from the European Union's Horizon Europe Framework Programme under grant agreement number 10105855 (NOVA).
Open access publication funding provided by COUPERIN CY26.
Contributor Information
Nihal Engin Vrana, Email: evrana@sparthamedical.eu.
Skander Hathroubi, Email: shathrou@sparthamedical.eu.
Data Availability Statement
The data that support the findings of this study are available from the corresponding author upon reasonable request.
References
- 1. ECDC. Healthcare‐Associated Infections: Surgical Site infections, Annual epidemiological report (2020), https://www.ecdc.europa.eu/sites/default/files/documents/healthcare‐associated‐infections‐intensive‐care‐units‐annual‐epidemiological‐report‐2020.pdf.
- 2. Leaper D. and Ousey K., “Evidence update on prevention of surgical site infection,” Current Opinion in Infectious Diseases 28, no. 2 (2015): 158–163, 10.1097/qco.0000000000000144. [DOI] [PubMed] [Google Scholar]
- 3. Bjarnsholt T., “The Role of Bacterial Biofilms in Chronic Infections,” Apmis 121 (2013): 1–58, 10.1111/apm.12099. [DOI] [PubMed] [Google Scholar]
- 4. Lichtenberg M., Kirketerp‐Møller K., Kvich L. A., et al., “Single Cells and Bacterial Biofilm Populations in Chronic Wound Infections,” Apmis 132 (2024): 1071–1077, 10.1111/apm.13344. [DOI] [PubMed] [Google Scholar]
- 5. Hathroubi S., Mekni M. A., Domenico P., Nguyen D., and Jacques M., “Biofilms: Microbial Shelters Against Antibiotics,” Microbial Drug Resistance 23 (2017): 147–156, 10.1089/mdr.2016.0087. [DOI] [PubMed] [Google Scholar]
- 6. Malone M., Bjarnsholt T., McBain A. J., et al., “The Prevalence of Biofilms in Chronic Wounds: A Systematic Review and Meta‐analysis of Published Data,” Journal of Wound Care 26 (2017): 20–25, 10.12968/jowc.2017.26.1.20. [DOI] [PubMed] [Google Scholar]
- 7. Lipsky B. A., Berendt A. R., Cornia P. B., et al., “2012 Infectious Diseases Society of America Clinical Practice Guideline for the Diagnosis and Treatment of Diabetic Foot Infectionsa,” Clinical Infectious Diseases 54 (2012): e132–e173, 10.1093/cid/cis346. [DOI] [PubMed] [Google Scholar]
- 8. Chávez‐Reyes J., Escárcega‐González C. E., Chavira‐Suárez E., et al., “Susceptibility for Some Infectious Diseases in Patients with Diabetes: The Key Role of Glycemia,” Frontiers in Public Health 9 (2021): 559595, 10.3389/fpubh.2021.559595. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 9. Joshi N., Caputo G. M., Weitekamp M. R., and Karchmer A. W., “Infections in Patients with Diabetes Mellitus,” New England Journal of Medicine 341 (1999): 1906–1912, 10.1056/nejm199912163412507. [DOI] [PubMed] [Google Scholar]
- 10. Ratliff C. R., Getchell‐White S. I., and Rodeheaver G. T., “Quantitation of Bacteria in Clean, Nonhealing, Chronic Wounds,” Wounds: A Compendium of Clinical Research and Practice 20 (2008): 279–283. [PubMed] [Google Scholar]
- 11. Thomas J. G., Motlagh H., Povey S. B., and Percival S. L., “2 ‐ The Role of Micro‐Organisms and Biofilms in Dysfunctional Wound Healing,” Advanced Wound Repair Therapies (Elsevier, 2011): 39–76, 10.1533/9780857093301.1.39. [DOI] [Google Scholar]
- 12. Finnegan S. and Percival S. L., “EDTA: An Antimicrobial and Antibiofilm Agent for Use in Wound Care,” Advances in Wound Care 4 (2015): 415–421, 10.1089/wound.2014.0577. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 13. Brandenburg K. S., Calderon D. F., Kierski P. R., et al., “Inhibition of Pseudomonas Aeruginosa Biofilm Formation on Wound Dressings,” Wound Repair and Regeneration 23 (2015): 842–854, 10.1111/wrr.12365. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 14. Edmiston C. E., Krepel C. J., Marks R. M., et al., “Microbiology of Explanted Suture Segments From Infected and Noninfected Surgical Patients,” Journal of Clinical Microbiology 51 (2012): 417–421, 10.1128/jcm.02442-12. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 15. Henry‐Stanley M. J., Hess D. J., Barnes A. M. T., Dunny G. M., and Wells C. L., “Bacterial Contamination of Surgical Suture Resembles a Biofilm,” Surgical Infections 11 (2010): 433–439, 10.1089/sur.2010.006. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 16. Novi V. T., Gonzalez A., Brockgreitens J., and Abbas A., “Highly Efficient and Durable Antimicrobial Nanocomposite Textiles,” Scientific Reports 12 (2022): 17332, 10.1038/s41598-022-22370-2. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 17. El Kalaaoui K., Bili O., Boukhriss A., et al., “Development of Antibacterial and Hydrophobic PVDF@ZnO Coating on Cotton Fabrics by Electrospinning Method,” Results in Surfaces and Interfaces 16 (2024): 100273, 10.1016/j.rsurfi.2024.100273. [DOI] [Google Scholar]
- 18. Meng X., Nan Q., Zeng Q., et al., “Antibacterial and Mothproofing Wool Fabrics Modified by M‐Arg/PHMG and ZnO,” Applied Surface Science 680 (2025): 161341, 10.1016/j.apsusc.2024.161341. [DOI] [Google Scholar]
- 19. Nešporová K., Pavlík V., Šafránková B., et al., “Effects of Wound Dressings Containing Silver on Skin and Immune Cells,” Scientific Reports 10 (2020): 15216, 10.1038/s41598-020-72249-3. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 20. Pang S., Gao Y., Wang F., et al., “Toxicity of Silver Nanoparticles on Wound Healing: A Case Study of Zebrafish Fin Regeneration Model,” Science of the Total Environment 717 (2020): 137178, 10.1016/j.scitotenv.2020.137178. [DOI] [PubMed] [Google Scholar]
- 21. Burd A., Kwok C. H., Hung S. C., et al., “A Comparative Study of the Cytotoxicity of Silver‐Based Dressings in Monolayer Cell, Tissue Explant, and Animal Models,” Wound Repair and Regeneration 15 (2007): 94–104, 10.1111/j.1524-475x.2006.00190.x. [DOI] [PubMed] [Google Scholar]
- 22. Zou S., Yoon W., Han S., Jeong S., Cui Z., and Kim W., “Cytotoxicity of Silver Dressings on Diabetic Fibroblasts,” International Wound Journal 10 (2013): 306–312, 10.1111/j.1742-481x.2012.00977.x. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 23. Poletti G., Mariani A., Brovarone S., et al., “Efficacy of Chlorhexidine‐Impregnated Dressings Compared to Standard Dressings in Preventing CLABSI/CRBSI and Catheter Colonization in Pediatric Patients: A Literature Review,” Hygiene, 5, no. 4 (2025): 59, 10.3390/hygiene5040059. [DOI] [Google Scholar]
- 24. Saeedi N. H., Alanazi A. D., Alenazy R., and Shater A. F., “Antimicrobial, Anti‐Inflammatory, Angiogenesis, and Wound Healing Activities of Copper Nanoparticles Green Synthesized by Lupinus arcticus Extract,” Iranian Journal Of Pharmaceutical Research 24, no. 1 (2025): 147434, 10.5812/ijpr-147434. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 25. Miao Z., Lu C., Xu C., et al., “A Small Library of Copper‐Based Metallenes with Superior Antibacterial Activity,” Materials Horizons 11, no. 22 (2024): 5564, 10.1039/d4mh01175a. [DOI] [PubMed] [Google Scholar]
- 26. Diao W., Li P., Jiang X., Zhou J., and Yang S., “Progress in Copper‐Based Materials for Wound Healing,” Wound Repair and Regeneration 32, no. 3 (2024): 314–322, 10.1111/wrr.13122. [DOI] [PubMed] [Google Scholar]
- 27. Conte M., Aliberti F., Fucci L., and Piscopo M., “Antimicrobial Activity of Various Cationic Molecules on Foodborne Pathogens,” World Journal of Microbiology and Biotechnology 23 (2007): 1679–1683, 10.1007/s11274-007-9415-6. [DOI] [PubMed] [Google Scholar]
- 28. Mutschler A., Tallet L., Rabineau M., et al., “Unexpected Bactericidal Activity of Poly(arginine)/Hyaluronan Nanolayered Coatings,” Chemistry of Materials 28 (2016): 8700–8709, 10.1021/acs.chemmater.6b03872. [DOI] [Google Scholar]
- 29. Gribova V., Boulmedais F., Dupret‐Bories A., et al., “Polyanionic Hydrogels as Reservoirs for Polycationic Antibiotic Substitutes Providing Prolonged Antibacterial Activity,” ACS Applied Materials & Interfaces 12 (2020): 19258–19267, 10.1021/acsami.9b23140. [DOI] [PubMed] [Google Scholar]
- 30. Kocgozlu L., Mutschler A., Tallet L., et al., “Cationic Homopolypeptides: A Versatile Tool to Design Multifunctional Antimicrobial Nanocoatings,” Materials Today Bio 28 (2024): 101168, 10.1016/j.mtbio.2024.101168. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 31. Tallet L., Gribova V., Ploux L., Vrana N. E., and Lavalle P., “New Smart Antimicrobial Hydrogels, Nanomaterials, and Coatings: Earlier Action, More Specific, Better Dosing?,” Advanced Healthcare Materials 10 (2021): 2001199, 10.1002/adhm.202001199. [DOI] [PubMed] [Google Scholar]
- 32. Frenkel J. S., “The Role of Hyaluronan in Wound Healing,” International Wound Journal 11 (2014): 159–163, 10.1111/j.1742-481x.2012.01057.x. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 33. Gribova V., Navalikhina A., Lysenko O., et al., “Prediction of Coating Thickness for Polyelectrolyte Multilayers via Machine Learning,” Scientific Reports 11, no. 1 (2021): 18702, 10.1038/s41598-021-98170-x. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 34. Šušteršič T., Gribova V., Nikolic M., Lavalle P., Filipovic N., and Vrana N. E., “The Effect of Machine Learning Algorithms on the Prediction of Layer‐by‐Layer Coating Properties,” ACS Omega 8, no. 5 (2023): 4677–4686, 10.1021/acsomega.2c06471. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 35. Özçelik H., Vrana N. E., Gudima A., et al., “Harnessing the Multifunctionality in Nature: A Bioactive Agent Release System with Self‐Antimicrobial and Immunomodulatory Properties,” Advanced Healthcare Materials 4 (2015): 2026–2036, 10.1002/adhm.201500546. [DOI] [PubMed] [Google Scholar]
- 36. Rowland M. B., Moore P. E., Bui C., and Correll R. N., “Assessing Wound Closure in Mice Using Skin‐Punch Biopsy,” STAR Protocols 4 (2023): 101989, 10.1016/j.xpro.2022.101989. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 37. Buček A., Popelka A., Zahoranová A., Kováčik D., Novák I., and Černák M., “Acrylic Acid Plasma Treatment of Polypropylene Nonwoven Fabric,” Fibres & Textiles in Eastern Europe 24 (2016): 161–164, 10.5604/12303666.1221751. [DOI] [Google Scholar]
- 38. Roque‐Borda C. A., Primo L. M. D. G., Medina‐Alarcón K. P., et al., “Antimicrobial Peptides: A Promising Alternative to Conventional Antimicrobials for Combating Polymicrobial Biofilms,” Advancement of Science 12 (2024): 2410893, 10.1002/advs.202410893. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 39. Mercer D. K., Katvars L. K., Hewitt F., Smith D. W., Robertson J., and O'Neil D. A., “NP108, an Antimicrobial Polymer with Activity Against Methicillin‐ and Mupirocin‐Resistant Staphylococcus aureus,” Antimicrobial Agents and Chemotherapy 61 (2017), 10.1128/aac.00502-17. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 40. Park S.‐C., Son H., Kim Y.‐M., et al., “Design of Antimicrobial Peptides with Cell‐Selective Activity and Membrane‐Acting Mechanism Against Drug‐Resistant Bacteria,” Antibiotics 11 (2022): 1619, 10.3390/antibiotics11111619. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 41. Lansdown A. B. G., “Silver I: Its Antibacterial Properties and Mechanism of Action,” Journal of Wound Care 11 (2002): 125–130, 10.12968/jowc.2002.11.4.26389. [DOI] [PubMed] [Google Scholar]
- 42. Thomas S. and McCubbin P., “An in Vitro Analysis of the Antimicrobial Properties of 10 Silver‐Containing Dressings,” Journal of Wound Care 12 (2003): 305–308, 10.12968/jowc.2003.12.8.26526. [DOI] [PubMed] [Google Scholar]
- 43. Pino P., Bosco F., Mollea C., and Onida B., “Antimicrobial Nano‐Zinc Oxide Biocomposites for Wound Healing Applications: A Review,” Pharmaceutics 15 (2023): 970, 10.3390/pharmaceutics15030970. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 44. Shrestha S., Wang B., and Dutta P. K., “Commercial Silver‐Based Dressings,” Vitro and Clinical Studies in Treatment of Chronic and Burn Wounds 13 (2024): 910, 10.3390/antibiotics13090910. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 45. Shah M. A., Pirzada B. M., Price G., Shibiru A. L., and Qurashi A., “Applications of Nanotechnology in Smart Textile Industry: A Critical Review,” Journal of Advanced Research 38 (2022): 55–75, 10.1016/j.jare.2022.01.008. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 46. De Jong W. H., Van Der Ven L. T. M., Sleijffers A., et al., “Systemic and Immunotoxicity of Silver Nanoparticles in an Intravenous 28 Days Repeated Dose Toxicity Study in Rats,” Biomaterials 34 (2013): 8333–8343, 10.1016/j.biomaterials.2013.06.048. [DOI] [PubMed] [Google Scholar]
- 47. Rezvani E., Rafferty A., McGuinness C., and Kennedy J., “Adverse Effects of Nanosilver on human Health and the Environment,” Acta Biomaterialia 94 (2019): 145–159, 10.1016/j.actbio.2019.05.042. [DOI] [PubMed] [Google Scholar]
- 48. Alshareef H. M., Abed Alharbi W., Khalaf N., et al., “Allergic Contact Dermatitis Caused by Silver Sulfate Present in the Wound Dressing Following Total Knee Arthroplasty: An Unusual Case,” Cureus 17, no. 5 (2025): 84351, 10.7759/cureus.84351. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 49. Yousefian F., Hesari R., Jensen T., et al., “Antimicrobial Wound Dressings: A Concise Review for Clinicians,” Antibiotics 12 (2023): 1434, 10.3390/antibiotics12091434. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 50. Charron R., Lemée P., Huguet A., et al., “Polyhexamethylene Biguanide Promotes Adaptive Cross‐Resistance to Gentamicin in Escherichia Coli Biofilms,” Frontiers in Cellular and Infection Microbiology 13 (2023): 1324991, 10.3389/fcimb.2023.1324991. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 51. ElDein M. A. T., Yassin A. S., El‐Tayeb O., and Kashef M. T., “Chlorhexidine Leads to the Evolution of Antibiotic‐Resistant Pseudomonas aeruginosa,” European Journal of Clinical Microbiology & Infectious Diseases 40 (2021): 2349–2361, 10.1007/s10096-021-04292-5. [DOI] [PubMed] [Google Scholar]
- 52. Yu F., Wang D., Zhang H., Wang Z., and Liu Y., “Evolutionary Trajectory of Bacterial Resistance to Antibiotics and Antimicrobial Peptides in Escherichia Coli,”. mSystems 10 (2025):e01700–e01724, 10.1128/msystems.01700-24. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 53. Hancock R. E. W., Alford M. A., and Haney E. F., “Antibiofilm Activity of Host Defence Peptides: Complexity Provides Opportunities,” Nature Reviews Microbiology 19 (2021): 786–797, 10.1038/s41579-021-00585-w. [DOI] [PubMed] [Google Scholar]
- 54. Zamboni F., Wong C. K., and Collins M. N., “Hyaluronic Acid Association With Bacterial, Fungal and Viral Infections: Can Hyaluronic Acid be Used as an Antimicrobial Polymer for Biomedical and Pharmaceutical Applications?,” Bioactive Materials 19 (2023): 458–473, 10.1016/j.bioactmat.2022.04.023. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 55. Parfenova L. V., Galimshina Z. R., Gil'fanova G. U., et al., “Hyaluronic Acid Bisphosphonates as Antifouling Antimicrobial Coatings for PEO‐modified Titanium Implants,” Surfaces and Interfaces 28 (2022): 101678, 10.1016/j.surfin.2021.101678. [DOI] [Google Scholar]
- 56. Eloïse L., Petit L., Nominé Y., et al., “The Antibacterial Properties of Branched Peptides Based on Poly(l‐arginine): In Vitro Antibacterial Evaluation and Molecular Dynamic Simulations,” European Journal of Medicinal Chemistry 268 (2024): 116224, 10.1016/j.ejmech.2024.116224. [DOI] [PubMed] [Google Scholar]
- 57. Roy R., Tiwari M., Donelli G., and Tiwari V., “Strategies for Combating Bacterial Biofilms: A Focus on Anti‐biofilm Agents and Their Mechanisms of Action,” Virulence 9 (2018): 522–554, 10.1080/21505594.2017.1313372. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 58. Huang H., Lai W., Cui M., et al., “An Evaluation of Blood Compatibility of Silver Nanoparticles,” Scientific Reports 6 (2016): 25518, 10.1038/srep25518. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 59. Krajewski S., Prucek R., Panacek A., et al., “Hemocompatibility Evaluation of Different Silver Nanoparticle Concentrations Employing a Modified Chandler‐Loop in Vitro Assay on Human Blood,” Acta Biomaterialia 9 (2013): 7460–7468, 10.1016/j.actbio.2013.03.016. [DOI] [PubMed] [Google Scholar]
Associated Data
This section collects any data citations, data availability statements, or supplementary materials included in this article.
Supplementary Materials
Supporting File: adhm70783‐sup‐0001‐SuppMat.docx.
Data Availability Statement
The data that support the findings of this study are available from the corresponding author upon reasonable request.