Abstract
Natural fibers are attractive, sustainable reinforcements, but often exhibit high moisture uptake and weak bonding with polymer matrices. In this study, jute and hemp were treated by immersion in aqueous calcium carbonate (CaCO3) suspensions (10–40 wt %, 1.5 h, room temperature) and were characterized by scanning electron microscopy (SEM), X-ray diffraction (XRD), moisture sorption testing, single-fiber tensile testing, and bundle pull-out testing. SEM showed granular CaCO3 deposition on fiber surfaces, with particulates bridging surface voids and microcracks. At 40 wt % CaCO3, equilibrium moisture uptake decreased to ∼5% (hemp) and ∼3% (jute), while tensile strength increased to ∼904 MPa (hemp) and ∼960 MPa (jute). Apparent interfacial shear strength from pull-out testing increased up to ∼1.35 MPa (hemp) and ∼0.56 MPa (jute). These results indicate that CaCO3 deposition is a mild, scalable surface treatment that improves moisture resistance, fiber tensile strength, and interfacial load transfer, relevant to semistructural composite applications, including interior and secondary automotive components.
Introduction
Natural fibers are increasingly used as sustainable reinforcements in polymer composites due to their low density, renewable nature, wide availability, and lower environmental footprint than conventional synthetic fibers such as glass or carbon. , Plant-derived fibers, including jute, hemp, flax, and kenaf, offer moderate strength and biodegradability, making them attractive for automotive − and construction , applications. Despite these advantages, large-scale adoption of natural fibers in structural composites remains limited by variability in source, quality, and consistency, as well as cost. These challenges are compounded by poor moisture resistance, heterogeneous microstructure and chemical composition, and weak interfacial bonding with polymer matrices. − The latter results in poor fiber wetting, reduced stress transfer at the interface, and diminished composite mechanical performance. As a result, composites reinforced with unmodified natural fibers often exhibit swelling, loss of mechanical integrity, and premature failure under moisture exposure, thermal cycling, UV degradation, or chemically aggressive environments. ,
To overcome these limitations, several studies have investigated a range of chemical treatments to modify fiber surface chemistry, improve fiber-matrix adhesion, and enhance the mechanical and thermal performance of natural fiber-reinforced composites. − Among them, alkali treatment with sodium hydroxide (NaOH) is one of the most widely applied methods. NaOH selectively removes noncellulosic constituents such as lignin, hemicellulose, pectin, waxes, and surface oils, , resulting in increased surface roughness, enhanced wettability, and reduced moisture absorption. These modifications significantly improve interfacial bonding and overall fiber mechanical performance. For instance, NaOH-treated jute has shown ∼37% higher tensile strength and improved modulus. Similarly, treated flax fibers exhibited reduced hemicellulose content and greater dimensional stability. However, NaOH effectiveness remains highly dependent on the treatment conditions. Overexposure above 10 wt % or prolonged durations can damage fibers, causing excessive fibrillation, cellulose degradation, surface erosion, and reduced structural integrity, as reported in cotton and bamboo fibers. ,
As an alternative to conventional alkali treatments, which can damage fibers under harsh conditions, calcium carbonate (CaCO3) offers a milder surface modification approach. Comparative studies on pineapple, flax, and fique fibers show that while NaOH improves tensile strength by ∼150% for fique and ∼40% for flax, CaCO3 treatment can achieve superior mechanical improvements for certain fibers, such as an ∼350% increase in pineapple fiber tensile strength. CaCO3 has also been shown to increase tensile modulus in kenaf fibers and improve dimensional stability in cotton by filling micropores. Additionally, CaCO3 is abundant, inexpensive, and environmentally friendly, making it a promising treatment for improving natural fiber performance.
While prior studies have demonstrated the potential of CaCO3 treatment for improving certain natural fibers, its effects across treatment concentrations and on widely used structural fibers such as jute and hemp remain insufficiently understood. In this letter, the influence of 10, 20, 30, and 40 wt % CaCO3 on the physical, chemical, and mechanical behavior of jute and hemp fibers is characterized. Fibers were soaked in CaCO3 suspensions at room temperature for 1.5 h, air-dried for 12 h, and then oven-dried at 80 °C for 2 h. The soaking duration was held constant to isolate the concentration effects across the treatment series. The sensitivity of deposition and property changes to the immersion time was not evaluated in this study. A detailed description of the materials and experimental methods is provided in the Supporting Information. Specifically, we examine how CaCO3 treatment concentration affects (1) surface morphology, (2) moisture sorption, (3) single-fiber mechanical properties, and (4) fiber-matrix interfacial bonding. The results provide a basis for optimizing CaCO3 treatment to enhance the performance of natural fiber-reinforced composites in structural applications.
Materials and Experimental Methods
Materials and Chemicals
Two commercially available natural fibers, hemp and jute, were obtained from Minifibers Inc. (USA), both with an average length of 130 mm. Calcium carbonate (CaCO3, powder; ACS reagent grade, ≥99.0% purity) was purchased from Sigma-Aldrich (USA). The fibers and chemical reagents were used as received without further processing.
Chemical Treatment of Natural Fibers
The treatment suspension was prepared by dispersing CaCO3 powder into deionized (DI) water at concentrations of 10, 20, 30, and 40 wt %. These concentrations were selected to systematically evaluate the effect of increasing the CaCO3 content in the suspension on natural fiber surface modification. Due to its low solubility in water, CaCO3 formed a heterogeneous suspension. Concentrations above 40 wt % were not considered, as higher solids content led to poor dispersion, excessive sedimentation, and increased viscosity.
Approximately 200 g of each fiber type was lightly brushed to remove any surface debris. Cleaned jute and hemp fibers were separately soaked in 10, 20, 30, and 40 wt % CaCO3 suspensions at ambient temperature for 1.5 h without agitation. After treatment, fibers were air-dried in a fume hood at room temperature for 12 h, then oven-dried at 80 °C for 2 h, and finally carefully stored in a sealed plastic bag. Fibers were not rinsed after treatment to retain surface-deposited mineral residues.
Mechanical Testing
Single-Fiber DMA Tensile Testing
Ten individual filaments from each fiber type, both untreated and chemically treated, were mounted on custom paper picture frames to facilitate handling during clamping. Fiber diameters were measured prior to testing by using a Keyence VR-5000 3D optical profilometer to enable accurate stress calculations. Tensile testing of the filaments was then conducted using a DMA Q800 (TA Instruments) following ASTM D3822 to determine the average tensile strength and Young’s modulus. The frames were carefully removed after the specimens were secured in the DMA grips. Tests were conducted at a gauge length of 15 mm and a constant strain rate of 5%/min. Prior to testing, the DMA was calibrated for force and displacement using the manufacturer’s standard procedures. Stress–strain data were recorded by using TA Instruments Universal Analysis 2000 software.
Fiber Pull-Out Testing
Similarly, fiber pull-out tests were conducted using DMA to evaluate the interfacial shear strength (IFSS) between the fibers and a polypropylene (PP) matrix. Specimens were prepared by embedding one end of a five-filament fiber bundle into a PP block (5 × 7 × 3 mm3, length × width × thickness), leaving 30 mm of exposed fiber length (Figure a). The free fiber end was clamped using tensile grips, while a custom 3D-printed fixture secured the PP block during loading. Following instrument calibration, tests were performed at a constant strain rate of 5%/min until interfacial debonding occurred. Five replicate specimens were tested per fiber type and treatment condition. During specimen preparation, five individual filaments were placed parallel across the silicone mold cavity and maintained straight or taut during PP deposition to preserve alignment along the loading axis. After solidification, excess PP was trimmed, and specimens were cut to a fixed embedded length (l = 5 mm). During testing, the PP block was constrained by using a 3D-printed fixture to minimize rotation and enforce axial loading. Because debonding can occur progressively across filaments, IFSS values are reported as apparent bundle-averaged quantities. Specimens exhibiting fiber breakage were excluded from IFSS extraction; only tests showing a clear interfacial pull-out response were used for the IFSS calculation.
1.

Experimental procedures used for fiber characterization: (a) interfacial shear strength (IFSS) testing setup and (b) cryofracture method used to prepare fibers for SEM imaging.
IFSS (τ, MPa) was calculated using
| 1 |
where F max is the maximum force (N), d is the fiber bundle diameter (mm), and l is the embedded fiber length in the PP matrix (mm).
Moisture Sorption Test
Moisture sorption capacity was evaluated for untreated and chemically treated hemp and jute fibers in accordance with ASTM C1104. Fiber samples (∼0.5 g each) were oven-dried at 80 °C for 2 h to remove residual moisture. The dried samples were placed on open trays in an environmental chamber maintained at 95% relative humidity and 30 °C. Fiber weight was recorded every 10 min using a digital balance (±0.0001 g) until mass equilibrium was reached (after ∼90 min; no measurable change between consecutive readings). Moisture sorption (M a, %) was calculated using
| 2 |
where W a and W d are the weights (g) of the moisture-saturated and oven-dried fibers, respectively.
Scanning Electron Microscopy
Fiber surface morphology was examined by scanning electron microscopy (SEM). Cross sections were prepared by cryofracturing: fibers were immersed in liquid nitrogen (−90 °C) for 30 s and mechanically fractured with tweezers, as shown in Figure b. For cross-sectional imaging, fibers were vertically mounted on pin stubs; for lateral surface imaging, fibers were placed horizontally. All samples were secured with conductive copper tape and sputter-coated with a 2 nm gold layer at 2.4 kV and 20 mA for 2 min. Imaging was performed using a JEOL JSM-IT500HR field-emission microscope at 1 kV beam voltage, PC 35, 12 mm working distance, and a 40 μm aperture. Micrographs were acquired at magnifications ranging from 500 to 10,000×.
Results and Discussion
SEM Characterization of Fiber Morphology
Figure shows scanning electron microscopy (SEM) micrographs of the lateral surfaces of untreated and 40 wt % CaCO3-treated hemp and jute fibers. In each case, the untreated fibers (Figure a,c) exhibited surface flaws, including longitudinal splits, microcracks, microvoids, and wall surface striations. These inherent defects likely formed during fiber growth, retting, mechanical separation, or drying. At higher densities, such flaws can act as stress concentrators, leading to premature crack initiation and fiber failure under mechanical loading. Following treatment, SEM micrographs acquired at multiple locations along the fiber axis showed consistent CaCO3 particulate coverage on the lateral surfaces, forming a granular coating that partially filled surface voids and bridged microcracks (Figure b, d). Full-length quantitative mapping of coating homogeneity was not performed; therefore, any local inhomogeneity along the gauge length could influence the tensile response. However, TGA indicated retained CaCO3 after treatment and showed that the apparent retained CaCO3 increased with suspension concentration, from 2.19 to 9.44 wt % for jute and from 11.60 to 16.16 wt % for hemp (Supporting Information, Figures S3–S4 and Table S3). These results are consistent with the SEM observations and confirm CaCO3 retention in the fibers after treatment.
2.
SEM micrographs of the lateral surfaces of (a, c) untreated and (b, d) 40 wt % CaCO3-treated hemp and jute fibers.
Natural fibers consist of a multilayered architecture comprising a primary wall, concentric secondary walls, and a central lumen. The lumen shape, size, and wall thickness vary by fiber type: jute typically exhibits thick-walled, oval-to-circular lumens, while hemp displays angular, irregular lumens. Figure shows SEM cross sections of untreated and 40 wt % CaCO3-treated hemp and jute fibers. Prior to imaging, individual filaments were cryofractured in liquid nitrogen to expose their internal morphology. In each untreated fiber (Figure a,c), the fracture surfaces appeared fragmented, with extensive microfibril pull-out, lumen collapse, and delamination of the wall layers. These failure features indicate weak interfibrillar cohesion, poor stress transfer, and a limited structural integrity. In contrast, after treatment, both fibers exhibited consolidated wall structures and well-defined lumen boundaries (Figure b,d). These morphological differences are consistent with improved wall cohesion after treatment (Figure b,d). Calcium ions (Ca2+) can form ionic bridges with pectic domains and other negatively charged polysaccharide functionalities in plant cell walls; such Ca2+-mediated cross-linking is widely reported in the literature to increase cohesion and reduce swelling/hydration-driven softening in plant-based materials. , Thus, Ca-containing species in the treatment environment may reinforce the cell wall network and suppress hydration-driven swelling, consistent with the measured strength increase and the reduced moisture uptake (Sections 2.2–2.3). In addition, CaCO3 particle deposition increased surface roughness, promoting mechanical interlocking at the fiber–matrix interface (Section 2.4).
3.
SEM micrographs of the cross sections of (a, c) untreated and (b, d) 40 wt % CaCO3-treated hemp and jute fibers.
Moisture Sorption
Moisture uptake compromises fiber integrity and weakens fiber–matrix bonding by promoting swelling, fibril separation, and increased porosity. In this work, moisture sorption was measured according to ASTM C1104 by placing oven-dried fiber samples in a controlled environment at 95% relative humidity and 30 °C for a single absorption exposure. Absorption–desorption hysteresis and humidity cycling were not evaluated. Equilibrium mass was reached within 90 min. Untreated hemp and jute fibers absorbed ∼68 and ∼30% moisture, respectively, relative to their oven-dried mass (Figure a). This high uptake arises primarily from hydroxyl-rich cellulose and hemicellulose domains that form hydrogen bonds with water molecules. Post-treatment, moisture uptake decreased significantly with increasing CaCO3 concentration (Figure a); at 40 wt %, uptake dropped to ∼5% for hemp and ∼3% for jute, corresponding to a >90% reduction from their untreated baseline. These results confirm that CaCO3 particle deposition formed a moisture-resistant barrier by filling microvoids and sealing wall cracks, which reduced the capillary pathways for water ingress.
4.
Comparison of untreated and CaCO3-treated hemp and jute fibers at 10–40 wt % concentrations. (a) Moisture sorption, (b) tensile strength, (c) tensile modulus, and (d) interfacial shear strength (IFSS).
Fiber Tensile Strength and Modulus
Single-fiber tensile testing was used to evaluate the effect of 10–40 wt % CaCO3 treatment on the tensile strength and modulus of hemp and jute fibers. The results are summarized in Table S1. For both fibers, strength generally increased with treatment concentration (Figure b). For instance, at 40 wt %, hemp strength increased from ∼498 to ∼904 MPa, and jute from ∼539 to ∼960 MPa, corresponding to ∼80% improvement over the untreated baselines. In contrast, changes in modulus were less pronounced: hemp increased slightly from ∼28 to ∼30 GPa, whereas jute decreased marginally from ∼56 to ∼53 GPa at 40 wt % CaCO3.
X-ray diffraction (XRD) confirmed cellulose I in both jute and hemp and revealed additional diffraction features consistent with crystalline CaCO3 after treatment. The crystallinity index (CI), quantified by peak deconvolution over 10–30°(2θ), decreased after 40 wt % CaCO3 treatment from 60.6 to 51.1% for jute and from 65.7 to 63.6% for hemp (Supporting Information, Figures S4–S6). This apparent decrease likely arises from overlap between CaCO3 reflections and cellulose peaks within the selected 2θ range used for CI estimation. Therefore, the CI values of the treated fibers cannot be used to determine whether the treatment altered the cellulose crystallinity or to assess any contribution of crystallinity to the observed strength increase. The strength increase is, instead, more consistent with microstructural and interfacial modifications introduced by the treatment. SEM showed CaCO3 particulates partially filling surface voids and bridging microcracks; treated fibers also exhibited reduced delamination and microfibril pull-out, consistent with lower local stress concentrations and delayed damage initiation. The reduced moisture uptake further supports improved resistance to water-induced swelling and interfacial degradation, which can otherwise promote microfibril debonding, increase local stress concentrations, and reduce fiber strength.
Notably, large standard deviations were observed in both the strength and modulus values, particularly at lower treatment concentrations. This variability likely reflects the inherent heterogeneity of natural fibers (e.g., wall thickness, defect density, lumen geometry), as well as batch-to-batch differences and possible local inhomogeneity in CaCO3 particle deposition. However, despite the scatter, the strength increase from untreated to 40 wt % CaCO3-treated fibers remained statistically significant for both hemp and jute (Welch’s two-sample t test, two-sided; hemp: p = 0.0026; jute: p = 0.0026; n = 10 per condition), and the difference in strength distributions is shown in the Supporting Information (Figures S2 and S3). These mechanical gains are consistent with the SEM observations of particulate deposition and defect bridging (Figure b,d), which can reduce local stress concentrations and improve load transfer.
Interfacial Shear Strength
Fiber pull-out tests were performed on nominal five-filament bundles embedded in polypropylene (PP) matrix blocks to evaluate interfacial shear strength (IFSS), using a DMA tensile fixture and a custom 3D-printed holder (see Supporting Information for setup and Figure a). Filaments were aligned parallel to the loading direction during embedding, and the embedded length was fixed (l = 5 mm). Because bundle testing can involve filament load sharing, the reported IFSS values represent bundle-averaged (“apparent”) interfacial performance and are used here for comparative assessment across treatment conditions under identical geometry and embedded length. PP was selected due to its low cost, thermal stability, and compatibility with natural fiber-reinforced composites. Untreated fibers exhibited low apparent IFSS of ∼0.55 MPa for hemp/PP and ∼0.20 MPa for jute/PP (Figure d), indicating weak fiber-matrix bonding and inefficient load transfer in the PP composite. The relatively higher apparent IFSS of hemp/PP compared to that of jute/PP reflects compositional and morphological differences between the two fibers. Hemp contains more cellulose and less lignin, offering greater surface reactivity and a more corrugated surface that promotes mechanical interlocking. In contrast, jute has higher lignin content and smoother, denser cell walls, which limit interfacial contact and reduce adhesion. In addition, surface-bound hemicellulose, waxes, and other polar impurities, combined with the hydrophilic nature of lignocellulosic fibers, likely reduced matrix wetting and hindered stress transfer. ,
In contrast, CaCO3-treated fibers exhibited markedly improved interfacial adhesion with the PP matrix due to treatment-induced surface morphological changes. Apparent IFSS is reported up to 30 wt % (Figure d); at 40 wt %, repeated fiber failure at the embedded-free fiber interface prevented reliable measurement. This suggests that, for the present pull-out geometry, the interfacial load transfer approached or exceeded the local fiber-cohesive strength, consistent with increased mechanical interlocking and elevated local stresses at the fiber-matrix interface. Accordingly, the 40 wt % condition is not interpreted as an ‘optimal’ IFSS case; rather, the dominant failure mode shifted from interfacial debonding to fiber breakage, precluding IFSS extraction. Modified embedded lengths and/or single-filament interfacial methods would be required to separate interfacial and fiber-cohesive contributions.
At 30 wt %, apparent IFSS increased to ∼1.35 MPa for hemp/PP and ∼0.56 MPa for jute/PP. As discussed previously, the granular CaCO3 coating increased surface roughness, improving micromechanical interlocking with the PP matrix. In addition, CaCO3 deposition and associated surface roughening likely improved local wetting and contact during PP melt infiltration, which can increase the apparent interfacial resistance to debonding in a nonpolar matrix. These results corroborate the tensile and SEM observations and are consistent with prior studies. ,,, The combined improvement in strength, interfacial bonding, and moisture resistance positions 40 wt % CaCO3-treated jute and hemp fibers as candidates for high-performance natural composite applications.
Conclusions
CaCO3 treatment significantly improved the structural performance of jute and hemp fibers through surface modification and lumen consolidation. At concentrations ≥30 wt %, tensile strength increased by ∼80% for both fibers, while interfacial shear strength improved by 145% in hemp/PP and 180% in jute/PP systems. Modulus changes were minimal, and moisture absorption decreased by more than 90%, indicating strong hydrophobic stabilization. The treatment process used mild conditions, with 1.5 h immersion at room temperature, followed by drying at 80 °C for 2 h, supporting scalability and low energy demand. CaCO3, therefore, provides a low-impact alternative to conventional alkali treatments, improving fiber strength and fiber-matrix adhesion without structural degradation. These results support its use in natural fiber-reinforced composites for structural applications. Future work will develop biobased resin composites reinforced with CaCO3-treated natural fibers.
Supplementary Material
Acknowledgments
This work was supported by the U.S. Department of Energy, Office of Energy Efficiency and Renewable Energy, Vehicle Technologies Office (EERE-VTO-DE-LC-000L078). The authors thank Rob Seffens, Jorge Ortiz, and Ethan Nickerson for their assistance with cryo-fracturing and tensile test preparation. The authors also thank Dr. Tanvi Ajantiwalay for assistance with SEM imaging. Schematic illustrations presented in this work were created by the authors using Adobe Illustrator.
The Supporting Information is available free of charge at https://pubs.acs.org/doi/10.1021/acsomega.6c00108.
Experimental setup for fiber pull-out testing; additional tensile strength box plots and statistical methods; XRD diffractograms and crystallinity index calculations; raw moisture sorption data; and additional SEM images (PDF)
The authors declare no competing financial interest.
References
- John R., Lin R., Jayaraman K., Bhattacharyya D.. Investigation on microstructure characteristics of tool wear and machined surface mechanisms while milling: kenaf vs glass fiber-reinforced composites. Journal of Materials Research and Technology. 2023;23:4716–4733. doi: 10.1016/j.jmrt.2023.02.115. [DOI] [Google Scholar]
- Mohanty A. K., Misra M., Hinrichsen G.. Biofibres, biodegradable polymers and biocomposites: An overview. Macromol. Mater. Eng. 2000;276–277(1):1–24. doi: 10.1002/(SICI)1439-2054(20000301)276:1<1::AID-MAME1>3.0.CO;2-W. [DOI] [Google Scholar]
- Salman S. D., Leman Z., Sultan M. T. H., Ishak M. R., Cardona F.. Influence of Fiber Content on Mechanical and Morphological Properties of Woven Kenaf Reinforced PVB Film Produced Using a Hot Press Technique. Int. J. Polym. Sci. 2016;2016(1):7828451. doi: 10.1155/2016/7828451. [DOI] [Google Scholar]
- Capretti M., Del Bianco G., Giammaria V., Boria S.. Natural Fibre and Hybrid Composite Thin-Walled Structures for Automotive Crashworthiness: A Review. Materials. 2024;17(10):2246. doi: 10.3390/ma17102246. [DOI] [PMC free article] [PubMed] [Google Scholar]
- Pickering K. L., Efendy M. G. A., Le T. M.. A review of recent developments in natural fibre composites and their mechanical performance. Composites Part A: Applied Science and Manufacturing. 2016;83:98–112. doi: 10.1016/j.compositesa.2015.08.038. [DOI] [Google Scholar]
- Volpe V., Pantani R.. Natural fiber-reinforced light composites for the automotive industry. Polym. Compos. 2025;46(9):8660–8673. doi: 10.1002/pc.29518. [DOI] [Google Scholar]
- Yusof N. S. B., Sapuan S. M., Sultan M. T. H., Jawaid M., Maleque M. A.. Design and materials development of automotive crash box: a review. Ciência & Tecnologia dos Materiais. 2017;29(3):129–144. doi: 10.1016/j.ctmat.2017.09.003. [DOI] [Google Scholar]
- Przybek A.. The Role of Natural Fibers in the Building IndustryThe Perspective of Sustainable Development. Materials. 2025;18(16):3803. doi: 10.3390/ma18163803. [DOI] [PMC free article] [PubMed] [Google Scholar]
- Kim, Y. K. ; Chalivendra, V. . 14 - Natural fibre composites (NFCs) for construction and automotive industries. In Handbook of Natural Fibres, 2nd edition; Kozłowski, R. M. ; Mackiewicz-Talarczyk, M. , Eds.; Woodhead Publishing, 2020; pp 469–498. [Google Scholar]
- Gholampour A., Ozbakkaloglu T.. A review of natural fiber composites: properties, modification and processing techniques, characterization, applications. J. Mater. Sci. 2020;55(3):829–892. doi: 10.1007/s10853-019-03990-y. [DOI] [Google Scholar]
- Mohammed M., Rahman R., Mohammed A. M., Adam T., Betar B. O., Osman A. F., Dahham O. S.. Surface treatment to improve water repellence and compatibility of natural fiber with polymer matrix: Recent advancement. Polym. Test. 2022;115:107707. doi: 10.1016/j.polymertesting.2022.107707. [DOI] [Google Scholar]
- Azwa Z. N., Yousif B. F., Manalo A. C., Karunasena W.. A review on the degradability of polymeric composites based on natural fibres. Materials & Design. 2013;47:424–442. doi: 10.1016/j.matdes.2012.11.025. [DOI] [Google Scholar]
- Valadez-Gonzalez A., Cervantes-Uc J. M., Olayo R., Herrera-Franco P. J.. Effect of fiber surface treatment on the fiber–matrix bond strength of natural fiber reinforced composites. Composites Part B: Engineering. 1999;30(3):309–320. doi: 10.1016/S1359-8368(98)00054-7. [DOI] [Google Scholar]
- Naveen J., Jawaid M., Zainudin E. S., Thariq Hameed Sultan M., Yahaya R.. Improved Mechanical and Moisture-Resistant Properties of Woven Hybrid Epoxy Composites by Graphene Nanoplatelets (GNP) Materials. 2019;12(8):1249. doi: 10.3390/ma12081249. [DOI] [PMC free article] [PubMed] [Google Scholar]
- Jayakrishna, K. ; Kar, V. R. ; Sultan, M. T. H. ; Rajesh, M. . 1 - Materials selection for aerospace components. In Sustainable Composites for Aerospace Applications; Jawaid, M. ; Thariq, M. , Eds.; Woodhead Publishing, 2018; pp 1–18. [Google Scholar]
- Chee S. S., Jawaid M., Sultan M. T. H.. Thermal stability and dynamic mechanical properties of kenaf/bamboo fibre reinforced epoxy composites. BioRes. 2017;12(4):7118–7132. doi: 10.15376/biores.12.4.7118-7132. [DOI] [Google Scholar]
- Ramachandran A., Mavinkere Rangappa S., Kushvaha V., Khan A., Seingchin S., Dhakal H. N.. Modification of Fibers and Matrices in Natural Fiber Reinforced Polymer Composites: A Comprehensive Review. Macromol. Rapid Commun. 2022;43(17):2100862. doi: 10.1002/marc.202100862. [DOI] [PubMed] [Google Scholar]
- Khalid M. Y., Imran R., Arif Z. U., Akram N., Arshad H., Al Rashid A., García Márquez F. P.. Developments in Chemical Treatments, Manufacturing Techniques and Potential Applications of Natural-Fibers-Based Biodegradable Composites. Coatings. 2021;11(3):293. doi: 10.3390/coatings11030293. [DOI] [Google Scholar]
- Elfaleh I., Abbassi F., Habibi M., Ahmad F., Guedri M., Nasri M., Garnier C.. A comprehensive review of natural fibers and their composites: An eco-friendly alternative to conventional materials. Results in Engineering. 2023;19:101271. doi: 10.1016/j.rineng.2023.101271. [DOI] [Google Scholar]
- Koohestani B., Darban A. K., Mokhtari P., Yilmaz E., Darezereshki E.. Comparison of different natural fiber treatments: a literature review. International Journal of Environmental Science and Technology. 2019;16(1):629–642. doi: 10.1007/s13762-018-1890-9. [DOI] [Google Scholar]
- Najeeb M. I., Sultan M. T. H., Andou Y., Shah A. U. M., Eksiler K., Jawaid M., Ariffin A. H.. Characterization of silane treated Malaysian Yankee Pineapple AC6 leaf fiber (PALF) towards industrial applications. Journal of Materials Research and Technology. 2020;9(3):3128–3139. doi: 10.1016/j.jmrt.2020.01.058. [DOI] [Google Scholar]
- Luchese C. L., Engel J. B., Tessaro I. C.. A Review on the Mercerization of Natural Fibers: Parameters and Effects. Korean Journal of Chemical Engineering. 2024;41(3):571–587. doi: 10.1007/s11814-024-00112-6. [DOI] [Google Scholar]
- Faruk O., Bledzki A. K., Fink H.-P., Sain M.. Biocomposites reinforced with natural fibers: 2000–2010. Prog. Polym. Sci. 2012;37(11):1552–1596. doi: 10.1016/j.progpolymsci.2012.04.003. [DOI] [Google Scholar]
- Belgacem, M. N. ; Gandini, A. . Natural fibre-surface modification and characterization. In Natural fibre reinforced polymer composites: from macro to nanoscale; CICEO, 2009; pp 14–46. [Google Scholar]
- Wang X., Chang L., Shi X., Wang L.. Effect of Hot-Alkali Treatment on the Structure Composition of Jute Fabrics and Mechanical Properties of Laminated Composites. Materials. 2019;12(9):1386. doi: 10.3390/ma12091386. [DOI] [PMC free article] [PubMed] [Google Scholar]
- Nwankwo C., Mahachi J., Olukanni D., Musonda I.. Alkali treatment of flax fibres: effects on tensile strength, thermal performance, and moisture absorption. Compos. Interfaces. 2025;32(9):1329–1346. doi: 10.1080/09276440.2025.2467700. [DOI] [Google Scholar]
- Moghassem A. R., Valipour P.. An extensive look into the effect of mercerization treatment on dimensional properties of cotton plain knitted fabric. Fibers Polym. 2013;14(2):330–337. doi: 10.1007/s12221-013-0330-1. [DOI] [Google Scholar]
- Zhang K., Wang F., Liang W., Wang Z., Duan Z., Yang B.. Thermal and Mechanical Properties of Bamboo Fiber Reinforced Epoxy Composites. Polymers. 2018;10(6):608. doi: 10.3390/polym10060608. [DOI] [PMC free article] [PubMed] [Google Scholar]
- Kaima J., Preechawuttipong I., Jongchansitto P., Charoenloe N.. Effect of Chemical Solution on Tensile Strength of Bamboo Fiber. IOP Conference Series: Materials Science and Engineering. 2020;886(1):012061. doi: 10.1088/1757-899X/886/1/012061. [DOI] [Google Scholar]
- Martínez Suárez C., Rojas Montejo P., Gutiérrez Junco O.. Effects of alkaline treatments on natural fibers. Journal of Physics: Conference Series. 2021;2046(1):012056. doi: 10.1088/1742-6596/2046/1/012056. [DOI] [Google Scholar]
- Liang K., Shi S., Wang G.. Effect of Impregnated Inorganic Nanoparticles on the Properties of the Kenaf Bast Fibers. Fibers. 2014;2(3):242–254. doi: 10.3390/fib2030242. [DOI] [Google Scholar]
- Wu Y., Dai M., Han Z., Wang Y., Xu W.. Effect of in-situ deposition of nano-calcium carbonate on the properties of anti-creasing cotton fabrics. Industrial Crops and Products. 2024;218:118931. doi: 10.1016/j.indcrop.2024.118931. [DOI] [Google Scholar]
- Chang V. S., Nagwani M., Kim C.-H., Holtzapple M. T.. Oxidative Lime Pretreatment of High-Lignin Biomass: Poplar Wood and Newspaper. Appl. Biochem. Biotechnol. 2001;94(1):01–28. doi: 10.1385/ABAB:94:1:01. [DOI] [PubMed] [Google Scholar]
- Shuvo I. I.. Fibre attributes and mapping the cultivar influence of different industrial cellulosic crops (cotton, hemp, flax, and canola) on textile properties. Bioresources and Bioprocessing. 2020;7(1):51. doi: 10.1186/s40643-020-00339-1. [DOI] [Google Scholar]
- Drouhet Q., Barbière R., Touchard F., Chocinski-Arnault L., Mellier D.. The Natural Growth of CaCO3 Crystals on Hemp Yarns: A Morphology Analysis and the Mechanical Effects on Composites. Fibers. 2023;11(10):88. doi: 10.3390/fib11100088. [DOI] [Google Scholar]
- Hubbe M. A., Sjöstrand B., Lestelius M., Håkansson H., Swerin A., Henriksson G.. Swelling of Cellulosic Fibers in Aqueous Systems: A Review of Chemical and Mechanistic Factors. BioResources. 2024;19(3):6859–6945. doi: 10.15376/biores.19.3.Hubbe. [DOI] [Google Scholar]; (acccessed 2026/03/03)
- Shubhra Q. T., Alam A., Quaiyyum M.. Mechanical properties of polypropylene composites: A review. Journal of Thermoplastic Composite Materials. 2013;26(3):362–391. doi: 10.1177/0892705711428659. [DOI] [Google Scholar]
- Alves Fidelis M. E., Pereira T. V. C., Gomes O. d. F. M., de Andrade Silva F., Toledo Filho R. D.. The effect of fiber morphology on the tensile strength of natural fibers. Journal of Materials Research and Technology. 2013;2(2):149–157. doi: 10.1016/j.jmrt.2013.02.003. [DOI] [Google Scholar]
- Herrera-Franco P. J., Valadez-González A.. A study of the mechanical properties of short natural-fiber reinforced composites. Composites Part B: Engineering. 2005;36(8):597–608. doi: 10.1016/j.compositesb.2005.04.001. [DOI] [Google Scholar]
Associated Data