Abstract
PURPOSE
This in vitro investigation was designed to assess the vertical marginal discrepancies in monolithic zirconia crowns manufactured using CAD-CAM technology, specifically focusing on the effects of progressive deterioration associated with the cumulative use of tungsten carbide instruments.
MATERIALS AND METHODS
Fifty-six monolithic zirconia crowns were manufactured utilizing a dry milling protocol. Milling was continued without bur replacement, and production proceeded with the same bur set even after the system issued a bur replacement warning after the 27th restoration. These restorations were then allocated into four distinct groups (n = 14 per group) based on the milling sequence. Marginal gap measurements were performed with a stereomicroscope, and measurements were obtained from the four surfaces of each crown. To evaluate statistical significance among the groups, a Welch analysis of variance (ANOVA) was conducted, followed by Games-Howell procedures for post hoc pairwise comparisons.
RESULTS
Significant variations in vertical marginal adaptation were detected among the tested cohorts (F = 68.5, P < .001). The mean ± SD (µm) values were as follows: G1 = 34.78 ± 5.89; G2 = 63.13 ± 14.53; G3 = 82.54 ± 17.61; and G4 = 99.69 ± 21.66. With the exception of Groups 3 and 4, which demonstrated statistically comparable outcomes (P = .126), all other pairwise comparisons yielded significant disparities. The marginal gap increased in parallel with the production sequence (r = 0.86, P < .001).
CONCLUSION
As the milling bur usage cycle increased, the marginal gap increased; however, the difference in marginal discrepancy between the later production groups (Group 3 and Group 4) was no longer statistically significant.
Keywords: Zirconium, Dental instruments, Computer-aided design, Computer-aided manufacturing, Dental marginal adaptation
INTRODUCTION
Marginal adaptation is widely regarded as one of the primary factors influencing the long-term biological and mechanical performance of fixed prosthetic restorations.1,2 Inadequate marginal fit has been associated with microleakage, secondary caries, and cement dissolution, all of which may compromise restoration longevity.3 Holmes et al.4 defined the parameters for measuring marginal gaps and proposed a value of ≤ 120 µm as the clinically acceptable threshold.
The utilization of CAD-CAM systems allows for the production of monolithic zirconia prostheses that exhibit superior mechanical durability, consistent esthetics, and high manufacturing precision.5 Nevertheless, the ultimate clinical adaptation of these milled restorations depends heavily on the condition of the milling instruments. Literature indicates that as cutting tools lose their geometric sharpness through repeated use, both the internal fit and marginal adaptation of the restorations may progressively deteriorate, potentially compromising their long term clinical performance.6 Use-related micro-wear of tungsten carbide burs may reduce material removal efficiency and surface precision, negatively affecting the marginal adaptation of restorations.7,8
Despite its clinical importance, limited data are available detailing how progressive deterioration associated with cumulative use influences the seating accuracy of these restorations. Consequently, the present in vitro investigation aimed to evaluate the impact of consecutive milling cycles on the vertical marginal discrepancies of CAD-CAM-machined monolithic zirconia crowns. The null hypothesis was that the deterioration associated with the cumulative use of tungsten carbide instruments would have no statistically significant effect on the vertical marginal discrepancy of the fabricated prostheses.
MATERIALS AND METHODS
In this study, a Frasaco AG-3 typodont (Frasaco GmbH, Tettnang, Germany) was selected, and the mandibular left first molar was prepared with a supragingival chamfer finish line (Fig. 1). A scanning spray (Vita Powder Scan Spray; VITA Zahnfabrik, Bad Säckingen, Germany) was applied to the prepared cast, which was subsequently digitized with a laboratory scanner (Ceramill Map 600 Plus; Amann Girrbach, Koblach, Austria) to capture the preparation margins. The resulting digital dataset served as the reference for the restoration design. From these scanned data, a die cast was fabricated using a three-dimensional (3D) printer (NextDent 5100; NextDent B.V., Soesterberg, The Netherlands) and its corresponding resin (NextDent Model 2.0; NextDent B.V.), following the manufacturer’s recommended workflow (Fig. 1). After fabrication, the cast was utilized for the try-in procedures and marginal adaptation assessment of the monolithic zirconia restorations.
Fig. 1. The prepared typodont jaw model and the corresponding die model, fabricated via additive manufacturing using scan data obtained from a laboratory scanner. The red arrows indicate the prepared tooth, while the yellow arrow highlights the preparation margin.

Monolithic zirconia crowns were fabricated using the Ceramill Motion 2 CAD-CAM system (Amann Girrbach, Koblach, Austria). To ensure absolute standardization, all 56 crowns were manufactured from a single, identical digital design file generated using CAD software (exocad DentalCAD; exocad GmbH, Darmstadt, Germany). The constant parameters applied to this master CAD file included a cement space of 40 µm, and a marginal thickness of 0.2 mm. Milling was performed using dedicated tungsten carbide burs (Ceramill Roto Motion Zr; Amann Girrbach) on multilayer monolithic zirconia blocks (Fusion Multilayer; Fusion Ceram B.V., Eindhoven, The Netherlands). To ensure surface consistency, the high-definition (HD) milling mode, representing the system’s highest precision setting, was utilized for all specimens.
A previously unused bur set was utilized to sequentially fabricate 56 crowns, which were allocated into four experimental groups (G1 – G4; n = 14 per group) based on the production sequence. The sample size of 14 specimens per group was chosen in accordance with similar in vitro studies evaluating the marginal adaptation of CAD-CAM restorations, which consistently report that sample sizes of 10 to 15 per group yield reliable statistical outcomes.9 During the milling of the 27th restoration, the CAM software generated a bur replacement warning for the 0.3-mm bur. This automated alert was triggered based on the manufacturer’s pre-set tool life algorithm, which calculates cumulative milling time and material volume, rather than real-time sensor feedback of physical bur wear. To simulate laboratory scenarios in which bur replacement is delayed despite system alerts, milling was continued without replacing the bur. Consequently, all restorations were produced using the same bur set (Fig. 2).
Fig. 2. Monolithic zirconia crowns fabricated sequentially using the same milling bur set. A total of 56 crowns were produced and arranged according to the production sequence, which was used to define the experimental groups (G1 – G4). This figure illustrates the progressive milling process without bur replacement.

Sintering was performed in a furnace (Ceramill Therm 3; Amann Girrbach). Furnace calibration was verified prior to sintering, and all specimens underwent a standardized thermal cycle according to the manufacturer’s parameters.
For the marginal gap measurements, each restoration was seated on the corresponding 3D-printed die. To simulate the initial clinical try-in procedure, seating was performed using firm finger pressure applied by a single operator to maintain consistency. Measurements were conducted in the production sequence using a stereomicroscope (Leica DFC320; Leica Microsystems Ltd., Heerbrugg, Switzerland) equipped with a light source (Leica CLS 150 XE; Leica Microsystems Ltd.) (Fig. 3). The vertical marginal gap values were obtained from digital images captured with the stereomicroscope, and the data were analyzed using image processing software (ImageJ; National Institutes of Health and the Laboratory for Optical and Computational Instrumentation [LOCI], University of Wisconsin, Madison, WI, USA) (Fig. 4). This optical evaluation method was utilized due to its established reliability for vertical discrepancy assessments. Additionally, due to the sequential nature of the experimental design and the measurement process, the operator performing the stereomicroscopic evaluations was not blinded to the group allocation. This lack of blinding may introduce a potential risk of observer bias and should be considered a methodological limitation of the present study.
Fig. 3. Direct measurement of the marginal fit of a zirconia crown seated on the die model under a stereomicroscope.

Fig. 4. Evaluation and measurement of vertical marginal discrepancy. (A) Stereomicroscopic view of the monolithic zirconia crown seated on the die during marginal gap assessment (Leica DFC320; Leica Microsystems Ltd., Heerbrugg, Switzerland). (B) ImageJ-based measurement of the vertical marginal gap at the crown-die interface. The measurement line represents the vertical discrepancy between the restoration margin and the preparation margin. Scale bar = 200 µm.

The marginal gap was defined as the vertical marginal discrepancy, in accordance with the criteria described by Holmes et al.4 Measurements were obtained from 15 points on each of the buccal, lingual, mesial, and distal surfaces of each crown, resulting in 60 measurement points per specimen and a total of 3,360 measurements. For the statistical analysis, these 60 measurements were averaged to compute a single overall mean marginal gap value for each crown. Additionally, surface-specific mean values were calculated to evaluate regional adaptations.
A schematic overview of the experimental procedures, from specimen preparation to marginal gap evaluation, is illustrated in Figure 5.
Fig. 5. Schematic illustration of the experimental workflow. The process involves scanning the prepared typodont model with a laboratory scanner, fabricating the die model via additive manufacturing using the scan data, designing the crown on the preparation representing tooth #36, and manufacturing the specimens via dry milling. Subsequently, direct marginal gap evaluation of the fabricated specimens is performed under a stereomicroscope, followed by the measurement of gap values in micrometers on the captured images using ImageJ software.

Statistical analyses of the data were performed using the jamovi software (Version 2.6.26; The jamovi project, Sydney, Australia). Descriptive statistics were calculated and reported as mean ± standard deviation for each group and surface. The normality of the data distribution was evaluated using the Shapiro-Wilk test, and the homogeneity of variances was assessed with Levene’s test. For data that met the assumption of normality but violated homoscedasticity, Welch’s ANOVA was utilized to determine overall significant differences, followed by the Games-Howell post hoc test for multiple pairwise comparisons. Conversely, for data that did not meet the assumption of normal distribution, the non-parametric Kruskal-Wallis test was employed. Subsequent pairwise comparisons for these datasets were conducted using Dunn’s post hoc test with Bonferroni correction. The level of statistical significance was set at P < .05 for all tests.
RESULTS
The mean marginal gap values were 34.78 ± 5.89 µm for Group 1, 63.13 ± 14.53 µm for Group 2, 82.54 ± 17.61 µm for Group 3, and 99.69 ± 21.66 µm for Group 4 (Table 1). Although the normality of the data was confirmed by the Shapiro-Wilk test (P > .05), the tested groups failed to demonstrate homoscedasticity (Levene’s test, P = .007). Welch’s ANOVA revealed significant differences in the mean marginal gap values among the groups (F = 68.5, P < .001). Games-Howell post hoc analysis demonstrated a progressive increase in the marginal gap values from Group 1 to Group 3, with no significant difference between Groups 3 and 4 (P = .126). These findings indicate that the increase in marginal gap values was no longer statistically distinguishable between the later production groups.
Table 1. The table presenting the mean marginal discrepancy and standard deviation values of the groups in micrometers (µm).
| Group | Buccal | Lingual | Mesial | Distal | Overall Mean |
|---|---|---|---|---|---|
| 1 | 37.45 ± 13.38 | 32.35 ± 7.15 | 33.67 ± 6.62 | 35.64 ± 4.80 | 34.78 ± 5.89 |
| 2 | 73.39 ± 17.63 | 55.04 ± 13.03 | 69.93 ± 34.44 | 54.17 ± 15.08 | 63.13 ± 14.53 |
| 3 | 98.68 ± 25.57 | 68.61 ± 17.72 | 80.54 ± 20.07 | 82.32 ± 26.78 | 82.54 ± 17.61 |
| 4 | 116.74 ± 25.60 | 71.62 ± 22.74 | 106.89 ± 28.94 | 103.49 ± 37.56 | 99.69 ± 21.66 |
Pearson correlation analysis showed a strong positive correlation between the fabrication sequence and marginal gap values (r = 0.86, P < .001), indicating a strong continuous increasing trend in the marginal gap with increasing bur usage.
The normality of data distribution for each specific surface was evaluated separately using the Shapiro-Wilk test. For the buccal surface, which met the normality assumption, Welch’s ANOVA was utilized, followed by Games-Howell post hoc tests. For the lingual, mesial, and distal surfaces, where the data violated the normality assumption, the non-parametric Kruskal-Wallis test was applied. Subsequent pairwise comparisons for these non-parametric surfaces were performed using Dunn’s post hoc test with Bonferroni correction to control for multiplicity. Surface-based analyses revealed that on the buccal surface (evaluated parametrically), Group 1 exhibited significantly lower marginal gap values compared to all other groups (P < .001). Additionally, Group 2 differed significantly from the final two groups, while the measurements for Groups 3 and 4 remained statistically equivalent (P > .05). For the surfaces analyzed using non-parametric tests, lingual evaluations indicated that Group 1 differed significantly from the remaining groups, which showed no significant differences among themselves. On the mesial surface, Group 1 differed significantly from all other groups; measurements for Groups 2 and 3 were statistically comparable, but both differed significantly from Group 4. Finally, distal evaluations revealed that Groups 1 and 2 each differed significantly from all other categories, whereas no statistical difference was observed between Groups 3 and 4 (Table 2).
Table 2. Group-based evaluation of marginal gap values.
| Pairwise comparisons | Buccal | Post hoc comparison P values | Distal | |
|---|---|---|---|---|
| Lingual | Mesial | |||
| G1-G2 | < .001 | < .001 | < .001 | .023 |
| G1-G3 | < .001 | < .001 | < .001 | < .001 |
| G1-G4 | < .001 | < .001 | < .001 | < .001 |
| G2-G3 | .027 | .149 | .235 | .008 |
| G2-G4 | < .001 | .149 | .008 | .002 |
| G3-G4 | .266 | 1.000 | .020 | .601 |
P < .05 was considered statistically significant.
P values indicating statistical differences between groups were derived from the Games-Howell post hoc test for the buccal surface, and Dunn’s post hoc test for the lingual, mesial, and distal surfaces.
DISCUSSION
The null hypothesis of the present in vitro investigation stated that the deterioration associated with the cumulative use of tungsten carbide burs would not significantly affect the marginal adaptation of monolithic zirconia crowns. The results demonstrated a progressive increase in the marginal gap values with an increasing production sequence, although the differences between the later production groups were no longer statistically significant. Accordingly, the null hypothesis was rejected.
These observations are consistent with the conclusions drawn by previous studies reporting that the sequential use of milling burs may adversely affect marginal adaptation. Raposo et al. demonstrated that the sequential use of diamond burs increased the marginal misfit of lithium disilicate crowns to a clinically relevant extent.10 Similarly, the present study demonstrated that the progressive use of tungsten carbide burs resulted in increased marginal gaps in monolithic zirconia crowns, indicating that the deterioration associated with cumulative use represents a common manufacturing-related factor affecting adaptation across different ceramic systems.
In digital workflows, scanning typodont or standardized reference casts to generate diagnostic casts has been reported as a repeatable and reliable method for evaluating accuracy in full-arch and single-crown studies.11 High-resolution laboratory scanning followed by physical cast fabrication with three-dimensional printing is utilized to support dimensional accuracy and data consistency.12 In the present study, rather than utilizing a standardized machined die, manual preparation on a Frasaco typodont followed by laboratory scanning was selected to evaluate marginal gaps. This approach was chosen to simulate clinical morphological details, such as axial convergence, chamfer finish lines, and surface finishing in the experimental model.
Previous investigations have reported that two-dimensional and three-dimensional measurement methods exhibit similar trends across many parameters; however, differences may arise in details, such as absolute marginal gap values and the precision of margin delineation, depending on the nature of the measurement approach. In the present study, only the vertical marginal discrepancy was evaluated to provide a direct and non-destructive assessment of the external restorative seal. While internal fit and absolute marginal discrepancy are also valuable adaptation parameters, they were not included as their assessment typically necessitates destructive sectioning of the specimens or advanced three-dimensional imaging techniques. Consequently, while general trends may coincide, exact numerical equivalence should not be expected.13
Stereomicroscopic image acquisition combined with digital image analysis (ImageJ) is widely reported as a valid and reproducible method for evaluating marginal fit. Values obtained through light microscopy have been validated against scanning electron microscopy (SEM) measurements, and comparable results have been reported with three-dimensional optical methods such as optical coherence tomography (OCT).14,15 Accordingly, direct marginal gap measurement using a stereomicroscope provides reliable two-dimensional data when standardized protocols are applied.16,17 However, the present study has several limitations. The use of a single tooth type, a specific preparation design, one monolithic zirconia material, and a single milling unit and bur system, along with a dry milling protocol and a single measurement approach, restricts the external validity of the findings. Additionally, although seating the crowns with firm finger pressure by a single operator improved consistency and simulated clinical conditions, the inability to apply a precisely quantified and mechanically standardized seating force is another valid limitation of this in vitro study. Future studies should incorporate diverse clinical scenarios and complementary three-dimensional evaluations.
Methodological reliability depends on the number of measurement points, clear definition of measurement geometry, and standardization of specimen positioning. Groten et al. reported that a higher number of measurement points per restoration increase the reliability.16 In the present study, 15 measurement points were obtained from each surface of each crown, yielding a total of 60 measurements per restoration. To avoid pseudoreplication within the statistical analysis, these multiple nested observations were not treated as independent data points. Instead, they were averaged to compute a single overall mean marginal gap value per crown, which served as the primary experimental unit for the global comparisons. Furthermore, surface-specific mean values were calculated separately for the regional analyses, ensuring that the statistical models correctly reflected the hierarchical structure of the data.
The integration of manual preparation on a typodont with subsequent digital scanning was utilized to incorporate clinical preparation features into a standardized digital workflow. This methodology aligns with established measurement protocols for evaluating marginal adaptation.11,18
The findings of this investigation reveal that the progressive utilization of milling instruments directly correlates with an increase in the marginal discrepancy of monolithic zirconia crowns. These observations are consistent with the conclusions drawn by Payaminia et al.,19 who also observed a negative effect of repeated bur use on restoration adaptation. Despite this increase, the mean marginal gap values across all groups remained below the clinically acceptable threshold of 120 µm proposed by Holmes et al.,4 indicating that a clinically acceptable level of manufacturing accuracy was maintained despite the deterioration associated with cumulative bur use.
Within the limitations of this in vitro study, the progressive deterioration associated with the cumulative use of milling burs was associated with an increase in the marginal discrepancy of monolithic zirconia restorations; however, the differences between the later production sequences were no longer statistically significant. Although all marginal gap values remained within clinically acceptable limits, these findings highlight the potential influence of instrument deterioration on manufacturing accuracy in CAD-CAM workflows. Monitoring bur usage and considering planned bur replacement strategies may help maintain optimal marginal adaptation during the fabrication of monolithic zirconia restorations.
CONCLUSION
Within the limitations of this in vitro study, the repeated use of tungsten carbide milling burs progressively increases the vertical marginal discrepancy of CAD-CAM monolithic zirconia crowns; however, this increase becomes statistically indistinguishable during later production stages. Furthermore, despite the deterioration associated with cumulative instrument use, all marginal gap values remain within clinically acceptable limits, indicating that the tested milling system maintains a clinically tolerable level of manufacturing accuracy even after extended service life.
Footnotes
This study was supported by the Scientific Research Projects Commission of Hatay Mustafa Kemal University (Project No: 24.DHU.008).
References
- 1.Memari Y, Mohajerfar M, Armin A, Kamalian F, Rezayani V, Beyabanaki E. Marginal adaptation of CAD/CAM all-ceramic crowns made by different impression methods: a literature review. J Prosthodont. 2019;28:e536–e544. doi: 10.1111/jopr.12800. [DOI] [PubMed] [Google Scholar]
- 2.Al-Humood H, Alfaraj A, Yang CC, Levon J, Chu TG, Lin WS. Marginal fit, mechanical properties, and esthetic outcomes of CAD/CAM interim Fixed Dental Prostheses (FDPs): a systematic review. Materials (Basel) 2023;16:1996. doi: 10.3390/ma16051996. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 3.Mounajjed R, Salinas TJ, Ingr T, Azar B. Effect of different resin luting cements on the marginal fit of lithium disilicate pressed crowns. J Prosthet Dent. 2018;119:975–980. doi: 10.1016/j.prosdent.2017.08.001. [DOI] [PubMed] [Google Scholar]
- 4.Holmes JR, Bayne SC, Holland GA, Sulik WD. Considerations in measurement of marginal fit. J Prosthet Dent. 1989;62:405–408. doi: 10.1016/0022-3913(89)90170-4. [DOI] [PubMed] [Google Scholar]
- 5.Leitão CIMB, Fernandes GVO, Azevedo LPP, Araújo FM, Donato H, Correia ARM. Clinical performance of monolithic CAD/CAM tooth-supported zirconia restorations: systematic review and meta-analysis. J Prosthodont Res. 2022;66:374–384. doi: 10.2186/jpr.JPR_D_21_00081. [DOI] [PubMed] [Google Scholar]
- 6.Liu X, Cameron AB, Haugli KH, Mougios AA, Heng NCK, Choi JJE. Influence of CAD/CAM diamond bur wear on the accuracy and surface roughness of dental ceramic restorations: a systematic review. J Mech Behav Biomed Mater. 2025;161:106813. doi: 10.1016/j.jmbbm.2024.106813. [DOI] [PubMed] [Google Scholar]
- 7.Hotta Y, Miyazaki T, Fujiwara T, Tomita S, Shinya A, Sugai Y, Ogura H. Durability of tungsten carbide burs for the fabrication of titanium crowns using dental CAD/CAM. Dent Mater J. 2004;23:190–196. doi: 10.4012/dmj.23.190. [DOI] [PubMed] [Google Scholar]
- 8.Oyar P, Ulusoy M, Durkan R. Effects of repeated use of tungsten carbide burs on the surface roughness and contact angles of a CAD-CAM PMMA denture base resin. J Prosthet Dent. 2022;128:1358–1362. doi: 10.1016/j.prosdent.2021.11.032. [DOI] [PubMed] [Google Scholar]
- 9.Doğan DG, Yaluğ ÖS. Marginal and internal fit of zirconia crowns with varying yttria content and finish line configurations: an in vitro study. Appl Sci. 2025;15:12440 [Google Scholar]
- 10.Raposo LH, Borella PS, Ferraz DC, Pereira LM, Prudente MS, Santos-Filho PC. Influence of Computer-aided Design/Computer-aided Manufacturing diamond bur wear on marginal misfit of two lithium disilicate ceramic systems. Oper Dent. 2020;45:416–425. doi: 10.2341/19-089-L. [DOI] [PubMed] [Google Scholar]
- 11.Ender A, Mehl A. In-vitro evaluation of the accuracy of conventional and digital methods of obtaining full-arch dental impressions. Quintessence Int. 2015;46:9–17. doi: 10.3290/j.qi.a32244. [DOI] [PubMed] [Google Scholar]
- 12.Németh A, Vitai V, Czumbel ML, Szabó B, Varga G, Kerémi B, Hegyi P, Hermann P, Borbély J. Clear guidance to select the most accurate technologies for 3D printing dental models - a network meta-analysis. J Dent. 2023;134:104532. doi: 10.1016/j.jdent.2023.104532. [DOI] [PubMed] [Google Scholar]
- 13.Hasanzade M, Koulivand S, Moslemian N, Alikhasi M. Comparison of three-dimensional digital technique with two-dimensional replica method for measuring marginal and internal fit of full coverage restorations. J Adv Prosthodont. 2020;12:173–180. doi: 10.4047/jap.2020.12.3.173. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 14.Villias AA, Kourtis SG, Karkazis HC, Polyzois GL. In vitro validation of Digital Image Analysis Sequence (DIAS) for the assessment of the marginal fit of cement-retained implant-supported experimental crowns. Int J Implant Dent. 2021;7:12. doi: 10.1186/s40729-021-00290-6. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 15.Groten M, Girthofer S, Pröbster L. Marginal fit consistency of copy-milled all-ceramic crowns during fabrication by light and scanning electron microscopic analysis in vitro. J Oral Rehabil. 1997;24:871–881. doi: 10.1046/j.1365-2842.1997.00592.x. [DOI] [PubMed] [Google Scholar]
- 16.Groten M, Axmann D, Pröbster L, Weber H. Determination of the minimum number of marginal gap measurements required for practical in-vitro testing. J Prosthet Dent. 2000;83:40–49. doi: 10.1016/s0022-3913(00)70087-4. [DOI] [PubMed] [Google Scholar]
- 17.Nawafleh NA, Mack F, Evans J, Mackay J, Hatamleh MM. Accuracy and reliability of methods to measure marginal adaptation of crowns and FDPs: a literature review. J Prosthodont. 2013;22:419–428. doi: 10.1111/jopr.12006. [DOI] [PubMed] [Google Scholar]
- 18.Rekow ED, Silva NR, Coelho PG, Zhang Y, Guess P, Thompson VP. Performance of dental ceramics: challenges for improvements. J Dent Res. 2011;90:937–952. doi: 10.1177/0022034510391795. [DOI] [PMC free article] [PubMed] [Google Scholar]
- 19.Payaminia L, Moslemian N, Younespour S, Koulivand S, Alikhasi M. Evaluating the effect of repeated use of milling burs on surface roughness and adaptation of digitally fabricated ceramic veneers. Heliyon. 2021;7:e06896. doi: 10.1016/j.heliyon.2021.e06896. [DOI] [PMC free article] [PubMed] [Google Scholar]