Skip to main content
. 2026 Aug 20;11(34):50853–50870. doi: 10.1021/acsomega.6c01931

3. Non-Isothermal DSC Test Data for Melting and Cooling Cycles of DPF/LLDPE Composites.

Samples Melting Temperature (Tm, °C) Crystallinity (%) Crystallization On-Set Temperature (T0, °C) Crystallization Peak Temperature (Tc, °C) Crystallization half time (s)
PE-single 126.90 40.00 117.40 112.73 28.02
PE/5F-single 126.70 41.12 117.95 112.45 33.00
PE/10F-single 126.62 39.86 118.36 112.59 34.62
PE/15F-single 126.37 33.50 118.65 112.73 35.52
PE/20F-single 126.56 33.78 118.91 112.60 37.86
PE-5F-double 126.85 39.80 118.10 112.45 33.84
PE-20F-double 126.51 33.10 118.64 112.31 38.00
5F-PE-double 127.10 40.51 118.50 112.18 37.92
20F-PE-double 126.73 35.50 118.86 112.30 39.36
PE-5F-PE-multi 127.00 39.93 117.81 112.18 33.78
PE-20F-PE-multi 126.70 35.66 118.36 112.31 36.30