Table 3.
u-HA/P(d/l)LA (wt ratio) | |||||
---|---|---|---|---|---|
0/100a | 50/50 | 60/40 | 70/30 | 80/20 | |
Sc (MPa) | 7.3±0.4 | 6.5±0.3 | 5.6±0.7 | 4.1±0.4 | 1.5±0.2 |
The interconnective porosity was 45–50% with an 110 μm average pore size.
u-HA/P(d/l)LA (wt ratio) | |||||
---|---|---|---|---|---|
0/100a | 50/50 | 60/40 | 70/30 | 80/20 | |
Sc (MPa) | 7.3±0.4 | 6.5±0.3 | 5.6±0.7 | 4.1±0.4 | 1.5±0.2 |
The interconnective porosity was 45–50% with an 110 μm average pore size.