Skip to main content
. 2010 May 5;2010:683962. doi: 10.1155/2010/683962

Table 1.

Comparison of mechanical properties, optical orientation and crystallinity index of A. pernyi silks, A. ventricosus spider dragline silk, and B. mori silk.

Silk Spinning speed (mm/s) Tensile strength (MPa) Initial modulus (GPa) Breaking energy ( × 105 J/kg) Strain at breaking Optical orientation (%) Crystallinity index
A. pernyi silk 10 386 4.6 0.75 0.56 27.2 0.69
25 403 5.0 0.61 0.37 36.0 0.73
28 408 5.5 0.81 0.50 37.4 0.74
52 483 7.2 0.63 0.32 39.4 0.76
68 567 8.7 0.73 0.31 41.5 0.80
95 639 9.9 1.04 0.40 46.4 0.84
100 564 7.9 0.84 0.37 54.0 0.77
Natural spinning 362 4.8 0.64 0.50 20.4 0.71

A. ventricosus spider dragline silk 10 1020 7.6 1.34 0.37

B. mori silk 10 400 4.0 0.76 0.35