Skip to main content
. Author manuscript; available in PMC: 2011 Dec 1.
Published in final edited form as: J Biomater Sci Polym Ed. 2011 Mar;22(10):1275–1298. doi: 10.1163/092050610X504260

Table 1.

Characteristics of ECT copolymers synthesized by ring opening copolymerization of ε-CL and TSU using mPEG (Mn=2,000 g/mol) as the initiator, and Sn(Oct)2 (0.1mol% of the hydroxyl group in mPEG) as the catalyst. The polymerization was carried out in bulk at 110 °C for 24 h.

ID Feed ratio (g) Yield (%) Polymer compositiona Mnb (kg/mol) Mwb (kg/mol) PDIb
PEG CL TSU
ECT0 1.0 10.0 0.0 87.3 EG113CL427 56.7 78.3 1.38
ECT2 1.0 8.0 2.0 85.2 EG113CL328TSU55 44.9 54.8 1.22
ECT5 1.0 5.0 5.0 78.2 EG113CL208TSU133 44.7 59.1 1.32
ECT10 1.0 0 10.0 57.4 EG113TSU261 44.0 58.9 1.34
a

Composition of CL and TSU calculated by 1H NMR.

b

Mn, Mw, and PDI (polydispersity index) determined by GPC.