Details of ball-milled SPS sample processing conditions, grain size and hardness.

sintering temperature (°C) dwell time (min) pressure (MPa) melting average grain size (µm) average hardness (Vickers)
1050 10 75 no 1.3 742
1050 10 100 no 1.2 754
1075 10 100 no 1.4 797
1100 10 75 slight 1.0 707
1150 3 75 yes 0.6 684