Table 3.

Results for the ultimate tensile strength evaluation (mean ± standard deviation) of biomodified demineralized dentin: effect of environmental challenges and treatment.

Ultimate tensile strength (MPa) of demineralized dentin: effect of environmental challenge
Environmental
challenge
Dentin treatment
Control 25% GD 6.5% GSE
24 hours 12.67 ± 4.92 B,a 8.98 ± 2.94C,a 16.78 ±3.58A,a
24 hours/collagenase 0.0 ± 0.0 C,c 10.54 ± 3.94B,a 17.12 ± 3.96A,a
8 months DW 4.73 (2.25)C,b 7.85 (3.22)B,a 12.13 (4.22)A,b

Different upper and lower case letters indicate statistically significant differences (p < 0.05) on each row and column, respectively.

DW: distilled water; GD: glutaraldehyde; GSE: grape seed extract