Skip to main content
. 2011 Feb 28;62(10):3575–3586. doi: 10.1093/jxb/err047

Table 4.

Wood anatomy in hybrid poplar stem (LS) after 46 days of treatment with different ozone concentrations

Treatment Tension wood
Opposite wood
Cambium cell layers (number) Fibre frequency (number mm−2) Vessel frequency (number mm−2) Vessel lumen diameter (μm) Cambium cell layers (number) Fibre frequency (number mm−2) Vessel frequency (number mm−2) Vessel lumen diameter (μm)
Control 6.4±0.5 2890±200 173±33 40.7±2.8 6.2±0.3 2970±200 200±13 49.8±3.1
Ozone, 50 nl l−1 ND 3760±510* 142±25* 47.4±1.2* ND 3120±480 179±12 49.7±3.6
Ozone, 100 nl l−1 ND 4560±730* 126±35* 45.1±4.5* ND 3340±410 220±27 49.1±1.3
Ozone, 200 nl l−1 3.3±0.4* 3790±170* 124±15* 47.2±2.6* 3.0±0.5* 3500±180 188±22 49.4±0.8
Ozone, 300 nl l−1 ND 4050±240* 105±62* 47.9±2.1* ND 3450±500 188±17 49.6±2.6

Data are mean values ±SD (n=3, individual replicates).

*Significant differences (P <0.05) between control and ozone treatments.

ND, not determined.