Table 1.
Synthesized PUU physical and mechanical properties
Intrinsic viscosity (dL/g) | Tensile strength at break (MPa) | Initial modulus (MPa) | Strain at break (%) | Permanent set (%) | Storage modulus(E′), 25–55°C | Loss modulus (E″), 25–55°C | |
---|---|---|---|---|---|---|---|
PUU-PCL2000 | 2.17±0.01 | 58.0±4.7 | 12.1±2.5 | 1192±102 | 677±30 | -* | -* |
| |||||||
PUU-PTMC1500 | 0.90±0.02 | 29.8±6.1 | 21.1±0.1 | 617±104 | 131±31 | 12.2 | 1.0 |
PUU-PTMC2500 | 1.74±0.02 | 47.0±7.8 | 12.2±1.2 | 831±75 | 149±12 | 8.6 | 0.7 |
PUU-PTMC5400 | 2.45±0.03 | 39.2±7.7 | 5.6±1.3 | 778±34 | 12±7 | 2.4 | 0.2 |
| |||||||
PUU-PVLCL2250 | 1.76±0.01 | 35.0±6.2 | 11.5±3.8 | 1295±150 | 132±1 | 5.2 | 0.4 |
PUU-PVLCL6000 | 2.75±0.01 | 29.3±5.2 | 2.8±1.3 | 1354±226 | 39±4 | 2.5 | 0.13 |
Data are mean +/− standard deviation
refer to Fig. 8a