Telodendrimers DOX/polymer (w/w, %) Particle size (nm)a DL (%) EE (%) DOX concentration in micellesb(mg/ml)
PEG5k-CA8 0 16 ± 3 N/A N/A N/A
5 15 ± 5 4.6 91 0.91
10 17 ± 7* 7.8 78 1.56
15 20 ± 9* 8.2 55 1.65
PEG2k-CA4 0 10 ± 2 N/A N/A N/A
5 10 ± 3 4.8 99 0.99
10 10 ± 4 9.7 97 1.94
15 12 ± 5 14.8 98 2.94
20 18 ± 6* 13.2 66 2.64
25 22 ± 8* 7.3 30 1.5
*

The sample was filtered through 0.22 μM filter due to the precipitation.

a

Data represent the mean ± standard deviation (n ± 3).

b

The telodendrimer concentration was kept at 20 mg/ml.