Table 4.

Three point flexural strength (σf) values for the experimental groups (MPa). Results presented as median (standard deviation), and statistical grouping (n=10).

Materials One Layer Two Layers Three Layers TRI
PT FT
YZ 861 (92)a 57.6 (7.6)e -----** 83.0 (9.9)d
IZ 401 (33)c 61.2 (9.1)e 412 (22)bc 63.5 (11.8)e
AL 474 (59)b 65.8 (15.8)e 414 (88)bc 63.0 (7.3)e
VM7 69.8 ± (12.0)e
VM9 65.5 ± (8.9)e
*

Values followed by the same letter are statistically similar (p≥0.05).

**

Quantitative data from YZ-FT group was not included in the statistical analysis.