Skip to main content
. 2012 Apr 10;13(4):4508–4522. doi: 10.3390/ijms13044508

Table 1.

Tensile properties of PCL/chitosan composite with different amounts of nano CaCO3.

Composite Tensile Strength (MPa) Elongation at Break (%) Modulus (MPa)
PCL/chitosan 15.05 ± 0.84 848.00 ± 6.87 160.26 ± 4.15
PCL/chitosan/0.5 wt% nano CaCO3 17.31 ± 0.92 915.00 ± 7.84 190.58 ± 3.20
PCL/chitosan/1 wt% nano CaCO3 20.18 ± 0.96 1215.00 ± 8.35 214.91 ± 3.53
PCL/chitosan/3 wt% nano CaCO3 14.65 ± 0.73 751.00 ± 6.54 231.80 ± 3.89
PCL/chitosan/5 wt% nano CaCO3 12.16 ± 0.67 460.00 ± 5.31 247.21 ± 5.36
PCL/chitosan/7 wt% nano CaCO3 9.18 ± 0.54 124.00 ± 4.57 278.60 ± 4.53