Skip to main content
. 2012 Jun 25;10:27. doi: 10.1186/1477-3155-10-27

Table 1.

Physicochemical properties of reaction steps in HNP formation using photon correlation spectroscopy (PCS), zeta potential measurement and inductively coupled plasma-optical emission spectroscopy (ICP-OES)

Particle
Hydrodynamic Radius nm ± SD
Polydispersity Index ± SD
Zeta Potential mV ± SD
Concentration determined by Inductively Coupled Plasma – Optical Emission Spectroscopy mgmL-1(Average value, n = 2)
        Fe Au
Fe3O4
1112 (97)
0.763 (0.104)
-16.9 (0.379)
14.5
-
Fe3O4-PEI
237 (2)
0.194 (0.030)
+55.6 (0.702)
13.5
-
Fe3O4-PEI-Auseed
309 (12)
0.363 (0.016)
+35.0 (0.115)
1.86
3.36
Fe3O4-PEI-Aucoat
132 (37)
0.792 (0.156)
-23.3 (1.950)
2.74
3.53
Fe3O4-PEI-Au-PEG 139 (71) 0.332 (0.072) -21.7 (0.551) 2.20 3.06